MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay FM® 680-1 Polyimide Film Adhesive
Categories: Polymer; Thermoset; Polyimide, TS; Polyimide, Thermoset Film

Material Notes: FM® 680-1 polyimide adhesive is a non-metallic version of FM 680 film adhesive designed for continuous service at temperature up to 700°F (371°C). FM 680-1 adhesive was specifically developed for radar transparent applications requiring extreme environmental durability. FM 680-1 adhesive is capable of bonding composite laminates and a wide variety of high temperature metallic substrates such as stainless steel and titanium while maintaining thermal oxidative stability. FM 680-1 adhesive is an excellent candidate for aircraft engine applications or for the bonding of new composite materials requiring co-cure or consolidation temperature up to 735°F (391°C). This adhesive is processible under standard manufacturing operations at temperatures as low as 600°F (316°C) and can handle freestanding post-cure up to 735°F (391°C). To achieve maximum performance in bonding prepared metallic details the use of BR® 680 primer is recommended. FM 680-1 adhesive is a non-aluminum-filled, condensation polyimide supported on fiberglass cloth. It is available in film, foam and paste forms. FM 680-1 adhesive utilizes the NR-150 B2 chemistry developed by DuPont.

Features & Benefits:

  • Radar transparent
  • 700°F (371°C) service temperature capability
  • Superior thermal oxidative stability
  • Condensation-type polyimide
  • 600°F (316°C) processing under standard manufacturing operations
  • Co-curable with Avimid® N and other polyimide composite materials
Applications:
  • Titanium bonding
  • Stainless steel bonding
  • Polyimide composite bonding

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Volatiles <= 18 %
Storage Temperature -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Shear Strength 625 psi
@Temperature 391 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 725 psi
@Temperature 391 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 750 psi
@Temperature 391 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 900 psi
@Temperature 24.0 °C
30 days immersion in JP-4 fuel at 120°F (49°C)
 900 psi
@Temperature 371 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 975 psi
@Temperature 24.0 °C
30 days at 160°F (71°C) and 100% RH
 1030 psi
@Temperature 360 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 1050 psi
@Temperature 371 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 1200 psi
@Temperature 371 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 1400 psi
@Temperature 360 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 1530 psi
@Temperature 337 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 1600 psi
@Temperature 343 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 1630 psi
@Temperature -55.0 °C
30 days at 160°F (71°C) and 100% RH
 1750 psi
@Temperature 316 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 1780 psi
@Temperature 288 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 2030 psi
@Temperature 316 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 2080 psi
@Temperature -55.0 °C
30 days immersion in JP-4 fuel at 120°F (49°C)
 2200 psi
@Temperature 337 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 2200 psi
@Temperature 177 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 2280 psi
@Temperature 24.0 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 2300 psi
@Temperature 288 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 2600 psi
@Temperature 288 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 2800 psi
@Temperature 177 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 2930 psi
@Temperature 260 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 2960 psi
@Temperature -55.0 °C
6AI-4V Titanium, Post-cure 16 hours at 700°F (371°C)
 3000 psi
@Temperature 177 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 3020 psi
@Temperature 24.0 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 3380 psi
@Temperature 24.0 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 3450 psi
@Temperature -55.0 °C
Avimid N Laminate, Post-cure 16 hours at 700°F (371°C)
 3550 psi
@Temperature -55.0 °C
6AI-4V Titanium, Post-cure 16 hours at 600°F (316°C)
 650 psi
@Temperature 338 °C,
Time 270000 sec
Thermal Exposure at 371°C
 650 psi
@Temperature 371 °C,
Time 270000 sec
Thermal Exposure at 371°C
 775 psi
@Temperature 343 °C,
Time 1.80e+6 sec
Thermal Exposure at 343°C
 950 psi
@Temperature 24.0 °C,
Time 270000 sec
Thermal Exposure at 371°C
 1100 psi
@Temperature 24.0 °C,
Time 900000 sec
Thermal Exposure at 343°C
 1130 psi
@Temperature 343 °C,
Time 900000 sec
Thermal Exposure at 343°C
 1200 psi
@Temperature 24.0 °C,
Time 1.80e+6 sec
Thermal Exposure at 343°C
 1230 psi
@Temperature 316 °C,
Time 3.96e+6 sec
Thermal Exposure at 316°C
 1600 psi
@Temperature 316 °C,
Time 900000 sec
Thermal Exposure at 316°C
 1650 psi
@Temperature 316 °C,
Time 7.20e+6 sec
Thermal Exposure at 316°C
 1650 psi
@Temperature 343 °C,
Time 450000 sec
Thermal Exposure at 343°C
 1650 psi
@Temperature 24.0 °C,
Time 7.20e+6 sec
Thermal Exposure at 316°C
 1850 psi
@Temperature 24.0 °C,
Time 3.96e+6 sec
Thermal Exposure at 316°C
 1850 psi
@Temperature 316 °C,
Time 1.80e+6 sec
Thermal Exposure at 316°C
 2100 psi
@Temperature 24.0 °C,
Time 450000 sec
Thermal Exposure at 343°C
 2130 psi
@Temperature 24.0 °C,
Time 900000 sec
Thermal Exposure at 316°C
 2240 psi
@Temperature 24.0 °C,
Time 1.80e+6 sec
Thermal Exposure at 316°C
 2250 psi
@Temperature 260 °C,
Time 3.60e+6 sec
Thermal Exposure at 260°C
 2330 psi
@Temperature 260 °C,
Time 2.07e+6 sec
Thermal Exposure at 260°C
 2350 psi
@Temperature 24.0 °C,
Time 7.20e+6 sec
Thermal Exposure at 260°C
 2380 psi
@Temperature 260 °C,
Time 7.20e+6 sec
Thermal Exposure at 260°C
 2550 psi
@Temperature 24.0 °C,
Time 2.07e+6 sec
Thermal Exposure at 260°C
 2680 psi
@Temperature 24.0 °C,
Time 3.60e+6 sec
Thermal Exposure at 260°C
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 371 °C
 
Processing PropertiesOriginal ValueComments
Shelf Life 6.00 Month
 
Descriptive Properties
ColorBrown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay FM® 680 Polyimide Film Adhesive
CEN® Electronic Material CV Polyimide Film, 1 Mil Thickness
Solvay FM® 680-2 Adhesive Foam
Cotronics Duralco™ 4703 Adhesive and Tooling Compound
Epoxy Technology EPO-TEK® 353ND High Temperature Epoxy

PCYTED061 / 180363

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.