MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2014-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Used in applications requiring high strength/hardness, including elevated temperature uses. Specific applications include heavy duty forgings, plate, and extrusions for aerospace fittings, wheels, tanks, and major structural components, heavy duty automotive frame and suspension componentry. 2014 exhibits poor corrosion resistance for an aluminum alloy.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
A Zr + Ti limit of 0.20 percent maximum may be used with this alloy designation for extruded and forged products only, but only when the supplier and the purchaser have mutually agreed.
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 2014-O; UNS A92014; ISO AlCu4SiMg; BS H15 (UK); CSA CS41N (Canada); AA2014-O, DIN AlCuSiMn; NF A-U4SG (France); Al2014-O
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.80 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 45AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 27.0 ksiAA; Typical
 <= 205 MPaExtruded wire, rod, bar, and shapes
 <= 205 MPaExtruded tube
 <= 220 MPa
@Thickness 0.508 - 12.7 mm
Sheet and plate
 <= 220 MPa
@Thickness 12.7 - 25.4 mm
Sheet and plate
 <= 220 MPa
@Thickness 4.57 - 12.7 mm
Drawn tube
Tensile Strength, Yield 14.0 ksiAA; Typical
 <= 125 MPaExtruded wire, rod, bar, and shapes
 <= 125 MPaExtruded tube
 <= 110 MPa
@Thickness 0.508 - 12.7 mm
Sheet and plate
 <= 110 MPa
@Thickness 4.57 - 12.7 mm
Drawn tube
Elongation at Break 12 %Extruded wire, rod, bar, and shapes
 12 %Extruded tube
 10 %
@Thickness 12.7 - 25.4 mm
Sheet and plate
 16 %
@Thickness 0.508 - 12.7 mm
Sheet and plate
 18 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Tensile Modulus 72.4 GPa
Compressive Strength 185 MPa
Compressive Modulus 73.8 GPa
Poissons Ratio 0.33
Fatigue Strength 13000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 30 %0-100 Scale of Aluminum Alloys
Shear Modulus 28.0 GPa
Shear Strength 18.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 21.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.8 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.880 J/g-°CEstimated from trends in similar Al alloys.
Thermal Conductivity 1340 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 945 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 945 °FAA; Typical
Liquidus 1180 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 935 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.4 - 95 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu 3.9 - 5.0 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.20 - 0.80 %
Manganese, Mn 0.40 - 1.2 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.50 - 1.2 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2014-T4; 2014-T451
Aluminum 2014-T6; 2014-T651
Aluminum 2014-T3
DWA 6092/SiC/17.5p-T6 Aluminum SiC Metal-Matrix-Composite (Al MMC), Sheet
Aluminum 2014-T6; 2014-T651 (Extended Form Data)

MA2014O / 8845

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.