System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Sumitomo Bakelite North America RX® 865M Novolac Phenolic
Categories:
Polymer
;
Thermoset
;
Filled/Reinforced Thermoset
;
Phenolic
;
Phenolic, Novolac, Glass Filled
Material Notes:
Fiberglass reinforced phenolic novolac compound featuring dimensional stability, moderate impact resistance, good strength and modulus.
Information provided by Vyncolit, a Sumitomo Bakelite Group
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Bulk Density
0.650
g/cc
Powder Density; ISO 60
Density
1.88
g/cc
Relative Density; ISO 1183
Linear Mold Shrinkage
0.0010
cm/cm
Compression Molding; ISO 2577
Mechanical Properties
Original Value
Comments
Hardness, Rockwell E
95
ISO 2039/2
Tensile Strength at Break
65.0
MPa
ISO 527
Flexural Strength
135
MPa
At Rupture; ISO 178
Flexural Modulus
20.0
GPa
ISO 178
Compressive Strength
265
MPa
ISO 604
Izod Impact, Notched (ISO)
4.50
kJ/m²
ISO 180
Electrical Properties
Original Value
Comments
Dielectric Strength
13.5
kV/mm
60Hz, Short Time, dry; ASTM D149
Arc Resistance
185
sec
ASTM D495
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
17.0
µm/m-°C
@Temperature 20.0 °C
ASTM E-831
CTE, linear, Transverse to Flow
39.0
µm/m-°C
@Temperature 20.0 °C
ASTM E-831
Thermal Conductivity
0.740
W/m-K
ASTM C-518
Maximum Service Temperature, Air
150
°C
UL 746B
Deflection Temperature at 1.8 MPa (264 psi)
>=
282
°C
Post Baked; ISO 75 A
Flammability, UL94
V-0
@Thickness 1.60 mm
V-0
@Thickness 3.20 mm
Descriptive Properties
Color
Black
Form
Flake
Main Filler
Glass Fiber
Molding Method
Compression, transfer, injection
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Sumitomo Bakelite North America 1907-1 / 1907B-1 Glass Reinforced Hardware Grade Epoxy
Sumitomo Bakelite North America 4064 Mineral Filled Electrical Encapsulation Grade Epoxy
Vyncolit X658 Novolac Phenolic
Sumitomo Bakelite North America 2-530 Short-Glass Reinforced Diallyl Phthalate
Sumitomo Bakelite North America 2008A Glass Reinforced Hardware Grade Epoxy
PVYNC022 / 72230
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.