MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Eastman DURASTAR DS2010 Natural PCTA Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP; PCTA Polyester Alloy; Polycyclohexylenedimethylene Terephthalate (PCT)

Material Notes: Application/Uses:
  • Appliances
  • Floor care
  • Refrigerator interior components
  • Toys/Sporting goods
  • Washing machine components
  • Writing instruments
Key Attributes:
  • Excellent clarity
  • Excellent flow
  • Fast drying times
  • Good chemical resistance
  • Outstanding impact resistance
  • Quick cycle times
Product Description: Durastar™ DS2010 polymer contains a mold release. It has excellent appearance and is nearly water-clear. Its most outstanding features are toughness, chemical resistance, and excellent processing characteristics. DS2010 has very good toughness as shown by Izod impact resistance. Exposure to aromatic oils often causes crazing or actual fracture of many polymer resins, but DS2010 maintains its physical properties when exposed to these oils, and its appearance is virtually unchanged. Easy to process, it flows readily and fills intricate molds. Under existing United States Food and Drug Administration (FDA) regulations, Durastar™ DS2010 may be used in food contact articles which comply with the specifications and conditions of use in 21 CFR 177.1240. This product is certified to ANSI/NSF Standard 51.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0020 - 0.0060 cm/cm
@Thickness 3.17 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 105ASTM D785
Tensile Strength at Break 49.0 MPaISO 527
Tensile Strength, Ultimate 53.0 MPaASTM D638
Tensile Strength, Yield 46.0 MPaASTM D638
 47.0 MPaISO 527
Elongation at Break 210 %ISO 527
 310 %ASTM D638
Elongation at Yield 4.0 %ISO 527
 5.0 %ASTM D638
Flexural Strength 64.0 MPaISO 178
Flexural Yield Strength 67.0 MPaASTM D790
Flexural Modulus 1.75 GPaISO 178
 1.90 GPaASTM D790
Izod Impact, Notched 3.70 J/cmASTM D256
 0.600 J/cm
@Temperature -40.0 °C
ASTM D256
Izod Impact, Notched (ISO) 6.30 kJ/m²
@Temperature -40.0 °C
ISO 180
 29.6 kJ/m²
@Temperature 23.0 °C
ISO 180
Impact Test NB
@Temperature 23.0 °C
ASTM D 4812
 NB
@Temperature -40.0 °C
ASTM D 4812
Puncture Energy 55.0 J
@Temperature -40.0 °C
Energy @ Max. Load; ISO 6603-2
 71.0 J
@Temperature 23.0 °C
Energy @ Max. Load; ISO 6603-2
 3763 J
@Temperature 23.0 °C
Energy @ Max. Load; ASTM D 3763
 3763 J
@Temperature -40.0 °C
Energy @ Max. Load; ASTM D 3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+17 ohm-cmASTM D 257
Surface Resistance 1.00e+17 ohmASTM D 257
Dielectric Constant 2.5
@Frequency 100000 Hz
ASTM D 150
 2.5
@Frequency 1e+6 Hz
ASTM D 150
 2.6
@Frequency 1000 Hz
ASTM D 150
 2.6
@Frequency 10000 Hz
ASTM D 150
Dielectric Strength 16.6 kV/mmShort Time, 500 V/sec rate of- rise; ASTM D 149
Dissipation Factor 0.0060
@Frequency 1000 Hz
ASTM D 150
 0.012
@Frequency 10000 Hz
ASTM D 150
 0.015
@Frequency 100000 Hz
ASTM D 150
 0.015
@Frequency 1e+6 Hz
ASTM D 150
Arc Resistance 123 secASTM D 495
Comparative Tracking Index 700 VASTM D 3638
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 73.0 °CASTM D648 and ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °CASTM D648
 66.0 °CISO 75
Flammability, UL94 V-2
@Thickness 3.00 mm
 
Optical PropertiesOriginal ValueComments
Haze 0.30 %ASTM D1003
Transmission, Visible 89 %Regular transmittance per ASTM D 1003
 91 %Total Transmittance; ASTM D 1003
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 - 290 °C
Mold Temperature 15.0 - 30.0 °C
Drying Temperature 70.0 °C
Dry Time 3.00 hour
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman DURASTAR DS1010 Natural PCTA Copolyester
A. Schulman Diamond NPP 60-1010 PCTA Polyester Alloy
Overview of materials for PCTA Polyester Alloy
Eastman DuraStar DS2110UVI Polymer, Natural
Eastman Eastar AN004 Natural PCTA Copolyester

PEA005 / 35219

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.