MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

(Viewing data as-entered. Click here to return)
Magnesium Elektron Elektron® AZ91 Magnesium Alloy
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: General purpose alloy. Good founding properties. Suitable for pressure die castings.

Information provided by Magnesium Elektron.

Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.83 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 60 - 75as sand cast
 60 - 75sand cast + solution treated
 85 - 100sand cast + solution and precipitation treated
Tensile Strength at Break 125 MPaSand cast
 170 MPaChill cast
 200 MPaSand cast, + solution treated
 200 MPaSand cast, solution treated and precipitation treated
 215 MPaChill cast, + solution treated
 215 MPaChill cast, solution and precipitation treated
Tensile Strength, Yield 80.0 MPa
@Strain 0.2 %
solution treated
 95.0 MPa
@Strain 0.2 %
Sand cast
 100 MPa
@Strain 0.2 %
Chill cast
 120 MPa
@Strain 0.2 %
solution and precipitation treated
Elongation at Break 2.0 %
 2.0 %Chill cast
 4.0 %Chill cast, + solution treated
 4.0 %Sand cast, + solution treated
 5.0 %Chill cast, solution and precipitation treated
Compressive Yield Strength 75.0 - 110 MPa
@Strain 0.2 %
solution and precipitation treated
 85.0 - 110 MPa
@Strain 0.2 %
as cast
 110 - 140 MPa
@Strain 0.2 %
solution and precipitation treated
Compressive Strength 185 - 432 MPaSolution treated
 280 - 340 MPaas cast
 385 - 465 MPasolution and precipitation treated
Fatigue Strength 58.0 - 62.0 MPa
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, solution and precipitation treated
 58.0 - 65.0 MPa
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, as cast
 65.0 - 77.0 MPa
@# of Cycles 5.00e+7
Rotating bend; semi-circular notch, radius 1.2 mm, solution treated
 70.0 - 77.0 MPa
@# of Cycles 5.00e+7
Unnotched Rotating Bend, solution and precipitation treated
 75.0 - 85.0 MPa
@# of Cycles 5.00e+7
Unnotched Rotating Bend, as cast
 77.0 - 92.0 MPa
@# of Cycles 5.00e+7
Unnotched Rotating Bend, solution treated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000141 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 27.0 µm/m-°C
@Temperature 20.0 - 200 °C
Specific Heat Capacity 1.00 J/g-°C
Thermal Conductivity 84.0 W/m-K
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 9.5 %
Magnesium, Mg 89.7 %As Balance
Manganese, Mn 0.30 %
Zinc, Zn 0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
SAE AZ91 Magnesium Matrix Composite, as cast
SAE SiC/AZ91 Magnesium Matrix Composite, as cast
Magnesium WE43-T6, Cast
Magnesium Elektron Elektron® AZ31B Magnesium Extrusion Alloy, UNS M11311
Magnesium AZ91D-F, Cast

NMAGEL940 / 186955

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.