MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilon® AG-30 LF 15 PA66-(GF+Z)45
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass Fiber/PTFE Filled

Material Notes: Product description: Grilon AG-30 LF 15 black 9832 is a heat stabilized, normal viscosity PA66 injection molding grade with 30% glass fibers and 15% of a combination of PTFE and silicone. Grilon AG-30 LF 15 black 9832 has the following important properties:
  • High stiffness
  • High wear resistance
  • Excellent sliding friction characteristics
Grilon AG-30 LF 15 black 9832 is used typically for slide bearing applications such as shaft bearing rings, gears and planetary gears.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.46 g/ccDry; ISO 1183
Water Absorption 5.0 %Sim. to ISO 62
Moisture Absorption 2.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 70.0 MPaConditioned; ISO 527-1/-2
 100 MPaDry; ISO 527-1/-2
Elongation at Break 4.0 %Dry; ISO 527-1/-2
 8.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 3000 MPaConditioned; ISO 527-1/-2
 6500 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched 30.0 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eU
 30.0 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
 40.0 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eU
 50.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
Charpy Impact, Notched 3.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 3.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 4.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 8.00 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 30.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-1/-2
Melting Point 260 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 110 °CLong Term; ISO 2578
 180 °CShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 190 °CISO 75-1/-2
Deflection Temperature at 8.0 MPa 70.0 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
AdditivesLubricants
AutomotiveAutomotive electr. and electronics, lighting
 Powertrain and Chassis
Electricals & ElectronicsElectrical appliances
FormGranules
Industry & Consumer goodsHeating systems
 Mechanical Engineering
 Power transmission
 Sports & Leisure
 Tools & Accessories
ProcessingInjection Molding
Product AttributesImproved friction & wear properties
Special CharacteristicsImproved heat resistance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Plastcom SLOVAMID 66 CF 30 PA66, 30% carbon fibre
EMS-Grivory Grivory® GV-6H PA*-GF60
EMS-Grivory Grilon® TSG-30/4 LF 15 PA666-(GF+Z)45
DuPont Mobility and Materials Zytel® FE270050 BK099 PA66-(GF+MD)30
DuPont Mobility and Materials Zytel® FE270038 BK267 PA66-(GF+MD)40

PGRH153 / 156862

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.