MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Makrolon® 1899 Polycarbonate, Impact Grade
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Impact Modified

Material Notes: MVR (300 °C/1.2 kg) 16 cm³/10 min; special flame retardent system; UL 94V-0/0.75 mm; impact modified; medium viscosity; easy release; vicat softening temperature 50 N; 50 °C/h = 110 °C; injection molding - melt temperature 240 - 280 °C; available in opaque colors only; battery housing

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.640 g/ccpellets; IOS 60
Density 1.20 g/ccISO 1183
Moisture Absorption at Equilibrium 0.12 %ISO 62
Water Absorption at Saturation 0.30 %ISO 62
Linear Mold Shrinkage, Flow 0.0060 cm/cm60x60x2 mm; 500 bar; ISO 294-4,2577
Linear Mold Shrinkage, Transverse 0.0065 cm/cm60x60x2 mm; 500 bar; ISO 294-4,2577
Melt Flow 17 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 60.0 MPa50 mm/min; ISO 527-1/-2
Tensile Strength, Yield 68.0 MPa50 mm/min; ISO 527-1/-2
Elongation at Break >= 50 %Nominal, 50 mm/min; ISO 527-1/-2
 115 %50 mm/min; ISO 527-1/-2
Elongation at Yield 4.8 %50 mm/min; ISO 527-1/-2
Tensile Modulus 2600 MPa1 mm/min; ISO 527-1/-2
Flexural Strength 100 MPa2 mm/min; ISO 178
Flexural Yield Strength 82.0 MPa
@Strain 3.5 %
2 mm/min; ISO 178
Flexural Modulus 2.60 GPa2 mm/min; ISO 178
Flexural Strain at Yield 5.8 %2 mm/min; ISO 178
Charpy Impact Unnotched NBISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/1eU
Impact 4500Puncture - maximum force (N); ISO 6603-2
 5400
@Temperature -30.0 °C
Puncture - maximum force (N); ISO 6603-2
Puncture Energy 50.0 JISO 6603-2
 55.0 J
@Temperature -30.0 °C
ISO 6603-2
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 100 VCTI M; Solution B; IEC 60112
 250 VIEC 60112
 250 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
Deflection Temperature at 0.46 MPa (66 psi) 105 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 96.0 °CISO 75-1/-2
Vicat Softening Point 110 °C50°C/h 50N; ISO 306
UL RTI, Electrical 80.0 °C
@Thickness 0.750 mm
UL 746B
UL RTI, Mechanical with Impact 80.0 °C
@Thickness 0.750 mm
UL 746B
UL RTI, Mechanical without Impact 80.0 °C
@Thickness 0.750 mm
UL 746B
Flammability, UL94 V-0
@Thickness 0.750 mm
IEC 60695-11-10
 5VA
@Thickness 3.00 mm
IEC 60695-11-20
Flash Point 460 °Cignition; ASTM D1929
 500 °Cself ignition; ASTM D1929
Oxygen Index 35 %ISO 4589-1/-2
Glow Wire Flammability Index 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °CInjection Molding; ISO 294
Mold Temperature 80.0 °CInjection Molding; ISO 294
Injection Velocity 200 mm/secISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LG Chemical LUPOY SC1004L PC, High Impact
Polyram RamTough PZ726 Polycarbonate, Impact Modified, UV Stabilized
Kingfa PC-S609 Toughened PC
A. Schulman Diamond PC 1035L Impact Modified, Polycarbonate, Injection Molding Grade
LG Chemical LI911 ASA

PB09895 / 92735

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.