MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Liquid Crystal Polymer (LCP), Mineral Filled
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Liquid Crystal Polymer (LCP), Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.52 - 1.89 g/ccAverage value: 1.70 g/cc Grade Count:32
Filler Content 30.0 - 50.0 %Average value: 40.0 % Grade Count:6
Water Absorption 0.0200 - 0.100 %Average value: 0.0380 % Grade Count:10
Moisture Absorption at Equilibrium 0.0200 - 0.0400 %Average value: 0.0233 % Grade Count:6
Linear Mold Shrinkage 0.000 - 0.00300 cm/cmAverage value: 0.00125 cm/cm Grade Count:26
Linear Mold Shrinkage, Transverse 0.00200 - 0.0110 cm/cmAverage value: 0.00568 cm/cm Grade Count:24
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 43.0 - 90.0Average value: 65.5 Grade Count:8
Tensile Strength, Ultimate 76.0 - 175 MPaAverage value: 128 MPa Grade Count:32
 48.0 - 200 MPa
@Temperature -40.0 - 150 °C
Average value: 86.6 MPa Grade Count:1
 17.0 - 216 MPa
@Temperature -40.0 - 250 °C
Average value: 86.6 MPa Grade Count:1
 17.0 - 216 MPa
@Thickness 1.60 - 3.17 mm
Average value: 86.6 MPa Grade Count:1
Elongation at Break 1.20 - 5.50 %Average value: 3.35 % Grade Count:30
 2.50 - 3.20 %
@Temperature 120 - 150 °C
Average value: 2.06 % Grade Count:1
 0.700 - 3.20 %
@Temperature -40.0 - 250 °C
Average value: 2.06 % Grade Count:1
 0.700 - 3.20 %
@Thickness 1.60 - 3.17 mm
Average value: 2.06 % Grade Count:1
Modulus of Elasticity 7.03 - 22.0 GPaAverage value: 11.9 GPa Grade Count:27
 4.80 - 11.6 GPa
@Temperature -40.0 - 150 °C
Average value: 7.45 GPa Grade Count:1
 2.77 - 16.5 GPa
@Temperature -40.0 - 250 °C
Average value: 7.45 GPa Grade Count:1
 2.77 - 16.5 GPa
@Thickness 1.60 - 3.17 mm
Average value: 7.45 GPa Grade Count:1
Flexural Yield Strength 87.0 - 230 MPaAverage value: 151 MPa Grade Count:29
 42.0 - 260 MPa
@Temperature -40.0 - 150 °C
Average value: 109 MPa Grade Count:2
 42.0 - 260 MPa
@Thickness 0.800 - 3.17 mm
Average value: 109 MPa Grade Count:2
Flexural Modulus 6.60 - 20.0 GPaAverage value: 11.5 GPa Grade Count:32
 3.30 - 16.7 GPa
@Temperature -40.0 - 150 °C
Average value: 7.38 GPa Grade Count:2
 3.30 - 16.7 GPa
@Thickness 0.800 - 3.17 mm
Average value: 7.38 GPa Grade Count:2
Flexural Strain at Break 2.00 - 2.40 %Average value: 2.23 % Grade Count:3
Compressive Yield Strength 51.7 - 131 MPaAverage value: 81.6 MPa Grade Count:8
Compressive Modulus 9.50 - 21.5 GPaAverage value: 14.1 GPa Grade Count:7
Izod Impact, Notched 0.500 - 1.60 J/cmAverage value: 0.996 J/cm Grade Count:5
Izod Impact, Notched (ISO) 5.00 - 60.0 kJ/m²Average value: 26.9 kJ/m² Grade Count:12
Charpy Impact Unnotched 2.10 - 8.40 J/cm²Average value: 5.64 J/cm² Grade Count:7
 4.00 - 4.00 J/cm²
@Temperature -30.0 - -30.0 °C
Average value: 4.00 J/cm² Grade Count:2
Charpy Impact, Notched 0.273 - 4.00 J/cm²Average value: 1.14 J/cm² Grade Count:24
 0.700 - 0.800 J/cm²
@Temperature -30.0 - -30.0 °C
Average value: 0.750 J/cm² Grade Count:2
Tensile Impact Strength 40.0 - 80.0 kJ/m²Average value: 56.7 kJ/m² Grade Count:3
Coefficient of Friction 0.120 - 0.210Average value: 0.172 Grade Count:4
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+12 - 2.50e+16 ohm-cmAverage value: 3.86e+15 ohm-cm Grade Count:18
Surface Resistance 3.10e+11 - 1.00e+17 ohmAverage value: 1.46e+16 ohm Grade Count:17
Dielectric Constant 2.90 - 6.70Average value: 3.81 Grade Count:17
 4.00 - 4.20
@Temperature 120 - 250 °C
Average value: 4.06 Grade Count:2
 4.00 - 4.20
@Frequency 1.00e+9 - 1.00e+10 Hz
Average value: 4.06 Grade Count:2
Dielectric Strength 22.0 - 66.0 kV/mmAverage value: 38.1 kV/mm Grade Count:10
Dissipation Factor 0.00100 - 0.0340Average value: 0.0133 Grade Count:16
 0.00500 - 0.0290
@Temperature 120 - 250 °C
Average value: 0.0149 Grade Count:2
 0.00500 - 0.0290
@Frequency 1.00e+9 - 1.00e+10 Hz
Average value: 0.0149 Grade Count:2
Arc Resistance 145 - 183 secAverage value: 174 sec Grade Count:8
Comparative Tracking Index 150 - 250 VAverage value: 199 V Grade Count:17
 
Thermal PropertiesOriginal ValueComments
CTE, linear -10.0 - 19.8 µm/m-°CAverage value: 6.87 µm/m-°C Grade Count:19
 18.0 - 18.0 µm/m-°C
@Temperature 20.0 - 180 °C
Average value: 8.91 µm/m-°C Grade Count:1
 -4.00 - 20.0 µm/m-°C
@Temperature 55.0 - 260 °C
Average value: 8.91 µm/m-°C Grade Count:3
 -4.00 - 20.0 µm/m-°C
@Thickness 2.00 - 4.00 mm
Average value: 8.91 µm/m-°C Grade Count:3
CTE, linear, Transverse to Flow 22.0 - 93.6 µm/m-°CAverage value: 44.2 µm/m-°C Grade Count:19
 88.2 - 100.8 µm/m-°C
@Temperature 20.0 - 180 °C
Average value: 52.0 µm/m-°C Grade Count:1
 34.0 - 62.0 µm/m-°C
@Temperature 55.0 - 260 °C
Average value: 52.0 µm/m-°C Grade Count:3
 34.0 - 62.0 µm/m-°C
@Thickness 2.00 - 4.00 mm
Average value: 52.0 µm/m-°C Grade Count:3
Specific Heat Capacity 0.000870 - 0.00138 J/g-°CAverage value: 0.00112 J/g-°C Grade Count:4
Thermal Conductivity 0.476 - 2.45 W/m-KAverage value: 0.988 W/m-K Grade Count:3
Melting Point 128 - 335 °CAverage value: 309 °C Grade Count:25
Maximum Service Temperature, Air 130 °CAverage value: 130 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 203 - 281 °CAverage value: 262 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 185 - 295 °CAverage value: 234 °C Grade Count:32
Vicat Softening Point 151 - 238 °CAverage value: 208 °C Grade Count:3
Glass Transition Temp, Tg 120 °CAverage value: 120 °C Grade Count:3
UL RTI, Electrical 130 - 240 °CAverage value: 161 °C Grade Count:12
UL RTI, Mechanical with Impact 130 - 220 °CAverage value: 156 °C Grade Count:12
UL RTI, Mechanical without Impact 130 - 240 °CAverage value: 185 °C Grade Count:6
Flammability, UL94 V-0Grade Count:21
Oxygen Index 40.0 - 47.0 %Average value: 43.5 % Grade Count:4
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 345 °CAverage value: 147 °C Grade Count:7
Nozzle Temperature 320 - 345 °CAverage value: 336 °C Grade Count:5
Die Temperature 290 - 360 °CAverage value: 333 °C Grade Count:5
Melt Temperature 270 - 399 °CAverage value: 334 °C Grade Count:22
Mold Temperature 30.0 - 160 °CAverage value: 92.5 °C Grade Count:18
Drying Temperature 149 - 170 °CAverage value: 151 °C Grade Count:20
Moisture Content 0.0100 %Average value: 0.0100 % Grade Count:12
Dew Point -40.0 - -28.9 °CAverage value: -32.6 °C Grade Count:3
Injection Pressure 50.0 - 200 MPaAverage value: 105 MPa Grade Count:11

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Liquid Crystal Polymer (LCP), Unfilled
Overview of materials for Liquid Crystal Polymer (LCP), 20% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), Carbon Fiber Filled

O2249 / 77950

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.