MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
TSE Industries Millathane® CM Millable Polyether Urethane Rubber with 60 PHR Suprex Clay Filler
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: MILLATHANE CM is a sulfur and peroxide curable polyether urethane rubber. Its outstanding property is its great resistance to abrasion, which makes it of special interest for articles that are subjected to high wear in service. It has a unique combination of excellent properties, such as low temperature characteristics, and resistance to heat deterioration, ozone cracking, weathering and swelling in oils or solvents.

All information provided by TSE Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.34 g/cc
Mooney Viscosity 13
@Temperature 121 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 59
Tensile Strength 2200 psi
Elongation at Break 725 %
100% Modulus 0.350 ksi
@Strain 100 %
300% Modulus 0.825 ksi
@Strain 300 %
Tear Strength 41.2 kN/mGraves
Compression Set 72 %Method B
 
Processing PropertiesOriginal ValueComments
Cure Time 90.0 min
@Temperature 142 °C
 
Descriptive Properties
Formulation as Tested0.35CAYTUR 4
 0.5Zinc Stearate
 0.75Sulfur
 1MBT
 100Millathane CM
 20Coumarone-Indene Resin
 4MBTS
 60Suprex Clay

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rogers Arlon 0.010" (0.254 mm) Flexible Heater Silicone with Fiberglass Substrate (49586R010)
Microcell Composite Company CELLOMER® 3000 SBS Rubber Pellets
LyondellBasell Petrothene® NA149000 Low Density Polyethylene, Sheet Extrusion Data
Austin Novel Materials Texalan® 770A PCL TPU
TSE Industries Millathane® E34 Millable Polyether Polyurethane Rubber with 0.5 PHR Sulfur

PMILL216 / 87260

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.