MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Schott AF 45 Thin Borosilicate Glass
Categories: Ceramic; Glass; Optical; Oxide; Silicon Oxide

Material Notes: AF 45 is an alkali-free modified borosilicate glass with a high content of BaO and Al2O3. AF 45, with its specific properties and large range of different thicknesses with tight tolerances, is exceptionally well suited for a number of applications including: liquid crystal displays, electroluminescent displays, CCD covers, hybrid circuits and solar cells. Due to a special down draw production process, AF 45 glass sheets have fire-polished surfaces; this glass type can be used without ground and polished surfaces. AF 45 offers excellent thermal resistance for high temperature applications up to approximately 600°C.

Information provided by SCHOTT North America.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.72 g/cc
Thickness 50.0 - 1100 microns
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 555HK100
Modulus of Elasticity 66.0 GPa
Poissons Ratio 0.235
Shear Modulus 26.7 GPa
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.60e+9 ohm-cm
@Temperature 500 °C
 3.20e+11 ohm-cm
@Temperature 350 °C
 6.00e+13 ohm-cm
@Temperature 250 °C
Dielectric Constant 6.2
@Frequency 1e+6 Hz
Dissipation Factor 0.00090
@Frequency 1e+6 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 4.50 µm/m-°C
@Temperature 20.0 - 300 °C
Thermal Conductivity 0.930 W/m-K
 1.04 W/m-K
@Temperature 87.0 °C
 1.10 W/m-K
@Temperature 127 °C
 1.13 W/m-K
@Temperature 166 °C
Maximum Service Temperature, Air 600 °C
Transformation Temperature, Tg 662 °C
Softening Point 883 °C107.6 dPa-s
Annealing Point 663 °C1013 dPa-s
Strain Point 627 °C1014.5 dPa-s
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.5255
@Wavelength 588 nm
nd
 1.5275
@Wavelength 546 nm
ne
Abbe Number 62.2νe
Optical Dispersion 0.0084nF - nC
Transmission, Visible 91.2 %
@Thickness 1.10 mm
 
Descriptive Properties
Stress Optical Coefficient3.2(1.02x10-12 m2/N

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
CeramTec Ceramtape GC Glass Ceramic
Schott KZFS12 Glass
Schott Glass 8241 Alkaline Earth Aluminosilicate Glass
Quartzite
Molybdenum, Mo; High Purity (UNS R03600)

CSGT0000 / 1985

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.