MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chemours Viton® A-331C Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Intermediate viscosity level (when compared with related ”O-Ring” polymers DuPont™ Viton® A-202C and DuPont™ Viton® A-402C)
  • Fully precompounded with reduced curative level and incorporated process aid
  • Improved processing with increased mold flow, better mold release with less mold fouling, and improved demolding ”hot tear”
  • Good compression set resistance

Applications

  • Injection, transfer and compression molding of:
    • O-rings, seals, and gaskets
    • Other profiles requiring improved demolding ”hot tear”
    • Extruded O-ring cord, hose, and other profiles

    Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.82 g/ccUncompounded Viton
Mooney Viscosity 65
@Temperature 121 °C
ML (1+10), Uncompounded Viton; ASTM D1646
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 71No Postcure; ASTM D2240
 7724 hours Postcure; ASTM D2240
Tensile Strength at Break 9.70 MPaNo Postcure; ASTM D412
 13.5 MPa24 hours Postcure; ASTM D412
Elongation at Break 237 %24 hours Postcure; ASTM D412
 351 %No Postcure; ASTM D412
100% Modulus 0.00310 GPa
@Strain 100 %
No Postcure; ASTM D412
 0.00450 GPa
@Strain 100 %
24 hours Postcure; ASTM D412
Compression Set 18 %
@Temperature 23.0 °C,
Time 252000 sec
O-Rings; ASTM D395B
 21 %
@Temperature 200 °C,
Time 252000 sec
O-Rings; ASTM D395B
 29 %
@Temperature 200 °C,
Time 605000 sec
O-Rings; ASTM D395B
 40 %
@Temperature 232 °C,
Time 252000 sec
O-Rings; ASTM D395B
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 204 °CContinuous use
 >= 260 °CIntermittent use
Minimum Service Temperature, Air -23.0 - -18.0 °CViton is generally useful down to -18 to -23°C.
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 °C
@Time 601 sec
Slab Cure
 232 °C
@Time 86400 sec
Postcure
 
Descriptive Properties
ColorOff-whiteUncompounded Viton
FormSheetUncompounded Viton
Formulation as Tested100A-331C
 3MgO
 30MT Black
 6Ca(OH)2
OdorNoneUncompounded Viton
Storage StabilityExcellentUncompounded Viton

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chemours Viton® B-303C Fluoroelastomer Compound
Chemours Viton® A-201C Fluoroelastomer (FKM)
Chemours Viton® A-700 Fluoroelastomer (FKM)
Chemours Viton® A-HV Fluoroelastomer (FKM)
Chemours Viton® A-361C Fluoroelastomer Compound

PDVC9887 / 170528

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.