MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics Steatite 22 Steatite
Categories: Ceramic; Oxide; Magnesium Oxide; Silicon Oxide

Material Notes: Good balance of electrical properties. Highly cost-effective for volume production of domestic component.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.50 - 2.80 g/ccFired
Porosity 0.00 %Apparent, fully dense
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell 45 N 67.1 - 70.6
Modulus of Elasticity 100 - 110 GPa
@Temperature 20.0 °C
Flexural Strength 125 - 126 MPa
@Temperature 20.0 °C
3-point
Compressive Strength 850 - 900 MPa
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1e+05 - 1.00e+6 ohm-cm
@Temperature 600 °C
 1.00e+13 - 1.00e+14 ohm-cm
@Temperature 20.0 °C
Dielectric Constant 6.1
@Frequency 1e+6 Hz
Dielectric Strength 24.0 - 26.0 kV/mm
@Temperature 20.0 °C
Dielectric Loss Index 0.00040 - 0.00060
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.90 - 8.60 µm/m-°C
@Temperature 20.0 °C
 7.90 - 8.60 µm/m-°C
@Temperature 800 °C
Specific Heat Capacity 0.900 J/g-°C
Thermal Conductivity 2.90 W/m-K
@Temperature 20.0 °C
Maximum Service Temperature, Air 1000 °C
 
Descriptive Properties
Thermal Downshock190Change in °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Du-Co Ceramics CS-144-L-5 Steatite
Morgan Advanced Ceramics Frequentite 1000 Steatite
Misumi Steatite
Du-Co Ceramics DC-16-L-3 Steatite
Morgan Advanced Ceramics 718U Steatite

CMORG46 / 90424

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.