System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
CoorsTek ACI-Co6 Tungsten Carbide
Categories:
Ceramic
;
Carbide
Material Notes:
Applications: seal rings, plungers, liners, nozzles, valve components, pump components, wear components in the oil & gas, construction, and agriculture equipment industries
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
14.9
g/cc
0.538
lb/in³
Particle Size
1.0
-
3.0
µm
1.0
-
3.0
µm
Grain Size
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell A
92
92
Modulus of Elasticity
627
GPa
90900
ksi
Flexural Strength
1930
MPa
280000
psi
Poissons Ratio
0.21
0.21
Shear Modulus
259
GPa
37600
ksi
Calculated
Thermal Properties
Metric
English
Comments
CTE, linear
4.70
µm/m-°C
@Temperature 25.0 - 400 °C
2.61
µin/in-°F
@Temperature 77.0 - 752 °F
5.30
µm/m-°C
@Temperature 25.0 - 800 °C
2.94
µin/in-°F
@Temperature 77.0 - 1470 °F
Specific Heat Capacity
0.2093
J/g-°C
0.05002
BTU/lb-°F
Thermal Conductivity
100
W/m-K
694
BTU-in/hr-ft²-°F
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
CoorsTek ACI-Co10 Tungsten Carbide
CoorsTek ACI-Ni6 Tungsten Carbide
CoorsTek ACI-Ni10 Tungsten Carbide
Tungsten Carbide, WC
Tungsten Carbide, W
2
C
CCOOR912 / 104616
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.