MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® 103FHSA NC010 PA66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Unreinforced, Heat Stabilized, Polyamide 66

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccDAM; ISO 1183
Melt Density 1.01 g/cc
@Temperature 290 °C
Water Absorption 8.5 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
 2.8 %
@Thickness 2.00 mm,
Time 86400 sec
Immersion; DAM; Sim. to ISO 62
Moisture Absorption 2.60 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 143 cm³/gDAM; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.014 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.013 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 121DAM; ISO 2039-2
Ball Indentation Hardness 85.0 MPaH 358/30; 50% RH; ISO 2039-1
 185 MPaH 358/30; DAM; ISO 2039-1
Tensile Strength, Yield 55.0 MPa50% RH; ISO 527-1/-2
 85.0 MPaDAM; ISO 527-1/-2
Elongation at Break 16 %Nominal; DAM; ISO 527-1/-2
 >= 50 %Nominal; 50% RH; ISO 527-1/-2
Elongation at Yield 4.5 %DAM; ISO 527-1/-2
 23 %50% RH; ISO 527-1/-2
Tensile Modulus 1400 MPa50% RH; ISO 527-1/-2
 3100 MPaDAM; ISO 527-1/-2
Flexural Strength 65.0 MPa
@Strain 3.5 %
50% RH; ISO 178
 95.0 MPa
@Strain 3.5 %
DAM; ISO 178
Flexural Modulus 1200 MPa50% RH; ISO 178
 2800 MPaDAM; ISO 178
Poissons Ratio 0.37DAM
 0.4350% RH
Izod Impact, Notched (ISO) 5.00 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 6.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 10.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 7.00 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour 1300 MPa1h; 50% RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 750 MPa1000h; 50% RH; ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+11 ohm-cm50% RH; IEC 62631-3-1
 1.00e+14 ohm-cmDAM; IEC 62631-3-1
Surface Resistance 1.00e+10 ohm50% RH; IEC 62631-3-2
Dielectric Strength 31.0 kV/mmDAM; IEC 60243-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 100 µm/m-°CDS; DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CDS; DAM; ISO 11359-1/-2
Specific Heat Capacity 2.79 J/g-°C
@Temperature 290 °C
Melt
Thermal Conductivity 0.160 W/m-K
@Temperature 290 °C
Melt
Melting Point 263 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 200 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 40.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 60.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 V-2
@Thickness 0.400 mm
DAM; IEC 60695-11-10
 V-2
@Thickness 1.50 mm
DAM; IEC 60695-11-10
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Glow Wire Test 700 °C
@Thickness 0.750 mm
No Flame; DAM; IEC 60335-1
 700 °C
@Thickness 1.00 mm
No Flame; DAM; IEC 60335-1
 700 °C
@Thickness 1.50 mm
No Flame; DAM; IEC 60335-1
 700 °C
@Thickness 2.00 mm
No Flame; DAM; IEC 60335-1
 700 °C
@Thickness 3.00 mm
No Flame; DAM; IEC 60335-1
Glow Wire Ignition Temperature 725 °C
@Thickness 0.400 mm
DAM; IEC 60695-2-12
 725 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-13
 725 °C
@Thickness 1.00 mm
DAM; IEC 60695-2-13
 725 °C
@Thickness 1.50 mm
DAM; IEC 60695-2-13
 725 °C
@Thickness 2.00 mm
DAM; IEC 60695-2-13
 725 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-13
Glow Wire Flammability Index 850 °C
@Thickness 0.400 mm
DAM; IEC 60695-2-12
 850 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 290 °COptimum, Injection
 280 - 300 °CRange, Injection
Mold Temperature 70.0 °COptimum, Injection
 50.0 - 90.0 °CInjection
Ejection Temperature 200 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
AdditivesRelease agent
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)5E-08
Emission of organic compounds (µgC/g)1.2VDA 277
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging (%)70F-value (refraction); ISO 6452; DAM
Fogging (mg)0.3G-value (condensate); ISO 6452; DAM
ISO designationISO 16396-PA66,,M1G1HNR,S14-030
Max. screw tangential speed (m/s)0.4Injection
Odor Class2.5VDA 270
Part Marking Code>PA66<ISO 11469
PolymerPA66
Processing Hold Pressure Time (s/mm)4Injection
Regional AvailabilityEurope
 Near East/Africa
Resin IdentificationPA66ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zytel® 151L NC010 PA612
Celanese Elvamide® 8061 PA6/66/610
DuPont Mobility and Materials Zytel® 103FHS BKB038 PA66
Celanese Zytel® 103HSL BKB080 PA66
Celanese Zytel® 101 NC010 PA66

PDSX5301 / 197941

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.