MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Bedford Plastics Glass Reinforced FR Polyester Structural Fiberglass Profiles
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Polyester, TS; Thermoset Polyester Glass SMC

Material Notes: Flame retardant grade; see details in the property table.

Pultrusion results in the production and supply of one of the worlds strongest and most durable products available today. The pultruded products feature:

  • High Strength
  • Corrosion Resistant to many chemicals
  • Light Weight- Weighs nearly 80% less than a steel profile of similar dimension
  • Electrically Non-Conductive
  • Non-Metallic
  • Lower Life Cycle Cost
  • Non-Leaching. Environmentally Friendly
  • Dimensional Stability

Information provided by Bedford Plastics.

Key Words: SMC; Fiber Reinforced Plastic (FRP)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.0620 - 0.0700 lb/in³ASTM D792
Water Absorption <= 0.45 %24 hrs; ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 45ASTM D2583
Tensile Strength, Ultimate 7000 psiCrosswise; ASTM D638
 30000 psiLengthwise; ASTM D638
Tensile Modulus 800000 psiCrosswise; ASTM D638
 2.50e+6 psiLengthwise; ASTM D638
Flexural Strength 10000 psiCrosswise; ASTM D790
 30000 psiLengthwise; ASTM D790
Flexural Modulus 800 ksiCrosswise; ASTM D790
 1800 ksiLengthwise; ASTM D790
Compressive Strength 15000 psiCrosswise; ASTM D635
 30000 psiLengthwise; ASTM D635
Compressive Modulus 1.00e+6 psiCrosswise; ASTM D635
 2.50e+6 psiLengthwise; ASTM D635
Shear Modulus 450 ksi
Shear Strength 4500 psiShort Beam Shear; ASTM D2344
 10000 psiPunch Shear; ASTM D732
Izod Impact, Notched 4.00 ft-lb/inCrosswise; ASTM D256
 25.0 ft-lb/inLengthwise; ASTM D256
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 5.0
@Frequency 60 Hz
Perpendicular to Laminate Face; ASTM D150
Dielectric Strength 35.0 kV/inLengthwise; ASTM D149
 200 V/milPerpendicular to Laminate Face; ASTM D149
Arc Resistance 120 secLengthwise; ASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.00 µm/m-°C
@Temperature 20.0 °C
Lengthwise; ASTM D696
Flame Spread Index <= 25Tunnel Test; ASTM E84
 
Descriptive Properties
FlammabilityNonburningASTM D635

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
E-Glass Fiber, Generic
Bedford Plastics Glass Reinforced Polyester Structural Fiberglass Profiles
Overview of materials for Low Carbon Steel
Bedford Plastics Glass Reinforced Vinylester Structural Fiberglass Profiles
Bedford Plastics Glass Reinforced Vinylester Flat Sheet, 3/16" to 1/4"

PBEDFO09 / 27106

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.