MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
309 Stainless Steel
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 300 Series Stainless Steel

Key Words: UNS S30900, ASME SA249, ASME SA312, ASME SA358, ASME SA403, ASME SA409, ASTM A167, ASTM A249, ASTM A312, ASTM A314, ASTM A358, ASTM A403, ASTM A409, ASTM A473, ASTM A511, ASTM A554, ASTM A580, FED QQ-S-763, FED QQ-S-766, MIL SPEC MIL-S-862, SAE J405 (30309), DIN 1.4828, X15CrNiSi2012, UNI X 16 CrNi 23 14, B.S. 309 S 24, PN 86022 (Poland), H20N13S2, austenitic
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.00 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 620 MPa
 76.0 MPa
@Temperature 980 °C
 105 MPa
@Temperature 925 °C
 145 MPa
@Temperature 870 °C
 185 MPa
@Temperature 815 °C
 250 MPa
@Temperature 760 °C
 305 MPa
@Temperature 705 °C
 380 MPa
@Temperature 650 °C
 405 MPa
@Temperature 595 °C
 455 MPa
@Temperature 540 °C
 475 MPa
@Temperature 480 °C
 495 MPa
@Temperature 425 °C
 510 MPa
@Temperature 370 °C
 515 MPa
@Temperature 315 °C
 530 MPa
@Temperature 260 °C
 550 MPa
@Temperature 205 °C
 560 MPa
@Temperature 150 °C
Tensile Strength, Yield 290 MPa
@Strain 0.2 %
 125 MPa
@Strain 0.2 %,
Temperature 870 °C
 130 MPa
@Strain 0.2 %,
Temperature 815 °C
 140 MPa
@Strain 0.2 %,
Temperature 760 °C
 145 MPa
@Strain 0.2 %,
Temperature 705 °C
 150 MPa
@Strain 0.2 %,
Temperature 650 °C
 160 MPa
@Strain 0.2 %,
Temperature 595 °C
 165 MPa
@Strain 0.2 %,
Temperature 540 °C
 170 MPa
@Strain 0.2 %,
Temperature 480 °C
 185 MPa
@Strain 0.2 %,
Temperature 425 °C
 195 MPa
@Strain 0.2 %,
Temperature 370 °C
 205 MPa
@Strain 0.2 %,
Temperature 315 °C
 220 MPa
@Strain 0.2 %,
Temperature 260 °C
 240 MPa
@Strain 0.2 %,
Temperature 205 °C
 255 MPa
@Strain 0.2 %,
Temperature 150 °C
Elongation at Break 50 %in 50 mm
 35 %
@Temperature 595 °C
in 50 mm
 35 %
@Temperature 650 °C
in 50 mm
 36 %
@Temperature 540 °C
in 50 mm
 37 %
@Temperature 705 °C
in 50 mm
 39 %
@Temperature 480 °C
in 50 mm
 40 %
@Temperature 425 °C
in 50 mm
 40 %
@Temperature 760 °C
in 50 mm
 43 %
@Temperature 370 °C
in 50 mm
 44 %
@Temperature 315 °C
in 50 mm
 45 %
@Temperature 260 °C
in 50 mm
 46 %
@Temperature 205 °C
in 50 mm
 46 %
@Temperature 815 °C
in 50 mm
 47 %
@Temperature 150 °C
in 50 mm
 50 %
@Temperature 870 °C
in 50 mm
 59 %
@Temperature 925 °C
in 50 mm
 65 %
@Temperature 980 °C
in 50 mm
Modulus of Elasticity 200 GPa
Poissons Ratio 0.30
Shear Modulus 77.0 GPa
Izod Impact 120 - 165 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000780 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.008at RT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.9 µm/m-°C
@Temperature 0.000 - 100 °C
 16.7 µm/m-°C
@Temperature 0.000 - 315 °C
 17.3 µm/m-°C
@Temperature 0.000 - 540 °C
 18.0 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.500 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 15.6 W/m-K
@Temperature 0.000 - 100 °C
Melting Point 1400 - 1455 °C
Solidus 1400 °C
Liquidus 1455 °C
Maximum Service Temperature, Air 980 °CIntermittent
 1095 °CContinuous Service
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.20 %
Chromium, Cr 23 %
Iron, Fe 60 %
Manganese, Mn <= 2.0 %
Nickel, Ni 14 %
Phosphorus, P <= 0.045 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
304 Stainless Steel
309 Stainless Steel, annealed, sheet
310 Stainless Steel, annealed sheet
301 Stainless Steel
Universal Wire Works 309 Stainless Steel Electrode

MQ309G / 12714

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.