MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Rhenium, Re; Annealed
Categories: Metal; Nonferrous Metal; Refractory Metal; Pure Element

Material Notes: Annealed applies only to tensile and/or hardness values; other property values are typical of the element. Stress relieving temperature 900-1200°C. Recrystallization temperature, 1 hour, is 1400-1600°C.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 21.03 g/cc
Vapor Pressure 1.00e-14 bar
@Temperature 1525 °C
 4.00e-11 bar
@Temperature 2000 °C
 1.10e-9 bar
@Temperature 2200 °C
 1.90e-8 bar
@Temperature 2400 °C
 1.60e-7 bar
@Temperature 2600 °C
 0.00000170 bar
@Temperature 2800 °C
 0.0000110 bar
@Temperature 3000 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 186.2071995
Atomic Number 75
Thermal Neutron Cross Section 86 barns/atom
X-ray Absorption Edge 0.17311 ÅK
 0.99009 ÅLI
 1.03645 ÅLII
 1.1772 ÅLIII
Electronegativity 1.9Pauling
Ionic Radius 0.560 ÅCrystal Ionic Radius for Valence +7
 0.720 ÅCrystal Ionic Radius for Valence +4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 165Converted from Vickers for 3000 kg load/10 mm ball Brinell test.
Hardness, Rockwell A 52Converted from Vickers.
Hardness, Rockwell B 85Converted from Vickers.
Hardness, Vickers 170
Tensile Strength, Ultimate 1070 MPa
 410 MPa
@Temperature 1200 °C
 620 MPa
@Temperature 800 °C
Tensile Strength, Yield 290 MPa
Elongation at Break 15 - 25 %
Modulus of Elasticity 469 GPa
Poissons Ratio 0.296
Shear Modulus 176 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000193 ohm-cm
@Temperature 20.0 °C
 0.0000254 ohm-cm
@Temperature 100 °C
 0.0000400 ohm-cm
@Temperature 300 °C
 0.0000526 ohm-cm
@Temperature 500 °C
 0.0000630 ohm-cm
@Temperature 700 °C
 0.0000725 ohm-cm
@Temperature 900 °C
 0.0000805 ohm-cm
@Temperature 1100 °C
 0.0000870 ohm-cm
@Temperature 1300 °C
 0.0000930 ohm-cm
@Temperature 1500 °C
 0.0000985 ohm-cm
@Temperature 1700 °C
 0.000103 ohm-cm
@Temperature 1900 °C
 0.0001065 ohm-cm
@Temperature 2100 °C
 0.000109 ohm-cm
@Temperature 2300 °C
Magnetic Susceptibility 3.63e-7cgs/g
Critical Magnetic Field Strength, Oersted 195 - 205
Critical Superconducting Temperature 1.691 - 1.703 K2.3 K max for Re II
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 178 J/g
CTE, linear 6.12 µm/m-°C
@Temperature 500 °C
 6.20 µm/m-°C
@Temperature 20.0 °C
 6.20 µm/m-°C
@Temperature 250 °C
 6.65 µm/m-°C
@Temperature 1000 °C
Specific Heat Capacity 0.134 J/g-°C
@Temperature 500 °C
 0.138 J/g-°C
@Temperature 25.0 °C
 0.150 J/g-°C
@Temperature 1000 °C
 0.161 J/g-°C
@Temperature 1000 °C
 0.177 J/g-°C
@Temperature 1500 °C
 0.199 J/g-°C
@Temperature 2000 °C
Thermal Conductivity 39.6 W/m-K
Melting Point 3180 °C
Boiling Point 5596 °C
Maximum Service Temperature, Inert 2380 °Cvaporization<1% after 10 hours
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.42
@Temperature 0.000 - 2000 °C,
Wavelength 655 nm
 
Component Elements PropertiesOriginal ValueComments
Rhenium, Re 100 %
 
Descriptive Properties
CAS Number7440-15-5

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rhenium, Re; Deformed
Rhodium, Rh; Annealed
Vanadium, V; Cold Rolled
Chromium, Cr; As-Swaged
Tantalum, Ta; Annealed

AMERe00 / 91

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.