MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Ensinger TECACOMP PEEK MED LDS grey 1067594 Polyetheretherketone, Mineral Reinforced
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK)

Material Notes:
  • developed for the LPKF-LDS® process
  • biocompatibility see declaration of conformity
  • very good chemical resistance
  • inherent flame retardant
  • good heat deflection temperature
  • low moisture absorption
Target Industries:
  • electrical engineering
  • mechanical engineering
  • medical technology
  • automotive industry

Information provided by Ensinger Inc.

Vendors: Ensinger TECACOMP compounds withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.65 g/cc
Water Absorption at Saturation 0.040 %50 % relative humidity up to saturation; DIN EN ISO 62
Linear Mold Shrinkage, Flow 0.0060 cm/cmDIN EN ISO 294-4
Linear Mold Shrinkage, Transverse 0.0060 cm/cmDIN EN ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 103 MPaDIN EN ISO 527-1
Elongation at Break 2.2 %DIN EN ISO 527-1
Modulus of Elasticity 10.7 GPaDIN EN ISO 527-1
Charpy Impact Unnotched 30.0 kJ/m²DIN EN ISO 179-1eU
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmDIN EN 61340-2-3
Surface Resistance 1.00e+14 ohmDIN EN 61340-2-3
Dielectric Constant 3.6
@Frequency 1e+9 Hz
Dissipation Factor 0.00060
@Frequency 1e+9 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 18.0 µm/m-°C
@Temperature 23.0 - 100 °C
DIN EN ISO 11359-1;2
 47.0 µm/m-°C
@Temperature 200 - 260 °C
DIN EN ISO 11359-1;2
 63.0 µm/m-°C
@Temperature 260 - 300 °C
DIN EN ISO 11359-1;2
CTE, linear, Transverse to Flow 31.0 µm/m-°C
@Temperature 23.0 - 100 °C
DIN EN ISO 11359-1;2
 87.0 µm/m-°C
@Temperature 200 - 260 °C
DIN EN ISO 11359-1;2
 110 µm/m-°C
@Temperature 260 - 300 °C
DIN EN ISO 11359-1;2
Specific Heat Capacity 0.800 J/g-°CDIN EN 821
Thermal Conductivity 0.500 W/m-Kthrough-plane; DIN EN 821
 1.20 W/m-Kin-plane; DIN EN 821
Melting Point 343 °CDIN 53765
Maximum Service Temperature, Air 260 °Clong term
 300 °Cshort term
Deflection Temperature at 1.8 MPa (264 psi) 254 °CISO-R 75 Method A
Glass Transition Temp, Tg 143 °CDIN 53765
Flammability, UL94 V-0
@Thickness 0.900 mm
DIN IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Processing Temperature 360 - 410 °C
Mold Temperature 170 - 210 °C
Drying Temperature 160 °C
Dry Time 4.00 hour
 
Descriptive Properties
Colorgrey
Thermal diffusivity0.28 mm2/sthrough-plane, DIN EN 821
 0.67 mm2/sin-plane, DIN EN 821

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PENSIO9091 / 319019

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.