MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2219-T31
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T31; AA2219-T31; Al2219-T31
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.84 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 100500 kg load with 10 mm ball
Hardness, Knoop 126Converted from Brinell Hardness Value
Hardness, Rockwell A 41.2Converted from Brinell Hardness Value
Hardness, Rockwell B 63Converted from Brinell Hardness Value
Hardness, Vickers 113Converted from Brinell Hardness Value
Tensile Strength, Ultimate 52.0 ksiAA; Typical
 >= 315 MPa
@Thickness 0.508 - 0.991 mm
Sheet
 >= 315 MPa
@Thickness 1.02 - 6.32 mm
Sheet
 >= 290 MPa
@Diameter <=12.7 mm
Wire, rod, bar, and shapes (extruded)
 >= 290 MPa
@Diameter <=12.7 mm
Extruded tube
 >= 310 MPa
@Diameter 12.7 - 76.17 mm
Wire, rod, bar, and shapes (extruded)
 >= 310 MPa
@Diameter 12.7 - 76.17 mm
Extruded tube
Tensile Strength, Yield 36.0 ksiAA; Typical
 >= 195 MPa
@Thickness 1.02 - 6.32 mm
Sheet
 >= 200 MPa
@Thickness 0.508 - 0.991 mm
Sheet
 >= 180 MPa
@Diameter <=12.7 mm
Wire, rod, bar, and shapes (extruded)
 >= 180 MPa
@Diameter <=12.7 mm
Extruded tube
 >= 185 MPa
@Diameter 12.7 - 76.17 mm
Wire, rod, bar, and shapes (extruded)
 >= 185 MPa
@Diameter 12.7 - 76.17 mm
Extruded tube
Elongation at Break 8.0 %
@Thickness 0.508 - 0.991 mm
Sheet
 10 %
@Thickness 1.02 - 6.32 mm
Sheet
 17 %
@Thickness 1.59 mm
AA; Typical
 14 %
@Diameter <=12.7 mm
Wire, rod, bar, and shapes (extruded)
 14 %
@Diameter 12.7 - 76.17 mm
Wire, rod, bar, and shapes (extruded)
 14 %
@Diameter <=12.7 mm
Extruded tube
 14 %
@Diameter 12.7 - 76.17 mm
Extruded tube
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Machinability 70 %0-100 Scale of Aluminum Alloys
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 250 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 37.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.864 J/g-°C
Thermal Conductivity 780 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 1010 °FAA; Typical
Liquidus 1190 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 995 °F
Aging Temperature 325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %
Iron, Fe <= 0.30 %
Magnesium, Mg <= 0.02 %
Manganese, Mn 0.20 - 0.40 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti 0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %
Zinc, Zn <= 0.10 %
Zirconium, Zr 0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2219-O
Aluminum 2219-T351
Aluminum 2219-T87
Aluminum 2219-T6
Aluminum 2219-T37

MA2219T31 / 8927

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.