MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® 70G30HSLR NC010 PA66-GF30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: 30% Glass Reinforced, Heat Stabilized, Hydrolysis Resistant, Polyamide 66

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccDAM; ISO 1183
Melt Density 1.20 g/cc
@Temperature 295 °C
Water Absorption 1.3 %
@Time 86400 sec
Immersion; DAM; Sim. to ISO 62
 6.0 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Moisture Absorption 1.90 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 150 cm³/gacid sulfuric 96%; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0030 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.011 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 8850% RH; ISO 2039-2
 104DAM; ISO 2039-2
Hardness, Rockwell R 11750% RH; ISO 2039-2
 124DAM; ISO 2039-2
Ball Indentation Hardness 185 MPaH 961/30; DS; 50% RH; ISO 2039-1
 270 MPaH 961/30; DS; DAM; ISO 2039-1
Tensile Strength at Break 130 MPa50% RH; ISO 527-1/-2
 200 MPaDAM; ISO 527-1/-2
Elongation at Break 3.3 %DAM; ISO 527-1/-2
 5.0 %50% RH; ISO 527-1/-2
Tensile Modulus 7000 MPa50% RH; ISO 527-1/-2
 10000 MPaDAM; ISO 527-1/-2
Flexural Strength 200 MPa50% RH; ISO 178
 280 MPaDAM; ISO 178
Flexural Modulus 6300 MPa50% RH; ISO 178
 9000 MPaDAM; ISO 178
Poissons Ratio 0.34DAM
 0.3550% RH
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 12.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 12.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 14.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Izod Impact, Unnotched (ISO) 60.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1U
 70.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1U
Charpy Impact Unnotched 70.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 70.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 70.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 80.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eU
Charpy Impact, Notched 10.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 10.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 10.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 12.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 15.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
Impact Test 5.00 J
@Thickness 2.00 mm
Multiaxial Impact, Total Energy; 4.5m/s; DAM; ISO 6603-2
Tensile Creep Modulus, 1 hour 6800 MPa1h; 50% RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 5100 MPa1000h; 50% RH; ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+11 ohm-cm50% RH; IEC 62631-3-1
 >= 1.00e+15 ohm-cmDAM; IEC 62631-3-1
Surface Resistance 1.00e+13 ohm50% RH; IEC 62631-3-2
Dielectric Constant 4.1
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
 4.3
@Frequency 100 Hz
DAM; IEC 62631-2-1
 4.6
@Frequency 1e+6 Hz
50% RH; IEC 62631-2-1
 11
@Frequency 100 Hz
50% RH; IEC 62631-2-1
Dielectric Strength 32.0 kV/mm50% RH; IEC 60243-1
 38.0 kV/mmDAM; IEC 60243-1
Dissipation Factor 0.0070
@Frequency 100 Hz
DAM; IEC 62631-2-1
 0.015
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
 0.065
@Frequency 1e+6 Hz
50% RH; IEC 62631-2-1
 0.46
@Frequency 100 Hz
50% RH; IEC 62631-2-1
Comparative Tracking Index 450 VDAM; IEC 60112
 400 - 599 V
@Thickness 3.00 mm
PLC 1; DAM; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 26.0 µm/m-°CDAM; ISO 11359-1/-2
 13.0 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
 26.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°CDAM; ISO 11359-1/-2
 70.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 130 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
Specific Heat Capacity 1.38 J/g-°CSolid; DS
 2.29 J/g-°C
@Temperature 295 °C
Melt
Thermal Conductivity 0.360 W/m-KSolid
 0.210 W/m-K
@Temperature 295 °C
Melt
Melting Point 262 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 261 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 253 °CDAM; ISO 75-1/-2
Vicat Softening Point 250 °C50°C/h, 50N; DAM; ISO 306
Glass Transition Temp, Tg 20.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 75.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 0.750 mm
DAM; IEC 60695-11-10
 HB
@Thickness 1.50 mm
DAM; IEC 60695-11-10
Flame Spread 24.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Oxygen Index 24 %DAM; ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 295 °COptimum, Injection
 285 - 305 °CRange, Injection
Mold Temperature 70.0 - 120 °CInjection
 100 °COptimum, Injection
Ejection Temperature 210 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
AdditivesRelease agent
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)1.1E-07
Emission of organic compounds (µgC/g)3.2VDA 277
FMVSS ClassSE/BISO 3795 (FMVSS 302)
Fogging (%)95F-value (refraction); ISO 6452; DAM
Fogging (mg)0.3G-value (condensate); ISO 6452; DAM
ISO designationISO 16396-PA66,GF30,M1GHNRW,S14-100
Max. screw tangential speed (m/s)0.2Injection
Odor Class4.5VDA 270
Part Marking Code>PA66-GF30<ISO 11469
PolymerPA66-GF30
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA66-GF30ISO 1043
Thermal desorption analysis of organic emissions (µg/g)5VDA 270

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zytel® 70G30L NC010 PA66-GF30
DuPont Mobility and Materials Zytel® 70G30HSL BK039B PA66-GF30
Celanese Zytel® 70G30HSLR BK099 PA66-GF30
DuPont Mobility and Materials Zytel® 70G30HSL NC010 PA66-GF30
Covestro Makrolon® 2458 Polycarbonate, Injection Grade

PDSX5326 / 197966

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.