MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BASF Ultramid® A3EG5 25% Glass Filled PA66 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: Glass fiber reinforced injection molding grade for machinery components and housings of high stiffness and dimensional stability such as coil formers and bearing cages. Also used for electrically insulating parts.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.500 - 0.800 g/cc
Density 1.32 g/ccISO 1183
Water Absorption 5.7 - 6.3 %ISO 62
Moisture Absorption at Equilibrium 1.7 - 2.1 %ISO 62
Viscosity Measurement 145ISO 307
Linear Mold Shrinkage 0.0055 cm/cm
Linear Mold Shrinkage, Flow 0.0048 cm/cmISO 2577
 0.0055 cm/cmTM=300°C, TW=80°C
Linear Mold Shrinkage, Transverse 0.0106 cm/cmISO 2577
Melt Flow 66 g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 175 MPaISO 527-1/-2
Elongation at Break 3.0 %ISO 527-1/-2
Modulus of Elasticity 8.60 GPaISO 527-1/-2
Flexural Strength 260 MPaISO 178
Flexural Modulus 7600 MPaISO 178
Izod Impact, Notched (ISO) 9.50 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Charpy Impact Unnotched 55.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 65.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 9.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 12.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Tensile Creep Modulus, 1000 hours 4300 MPa
@Strain <=0.5 %
ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Dielectric Constant 3.5
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.014
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 550 VTest Solution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 25.0 - 35.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 60.0 - 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-1/-2
Thermal Conductivity 0.340 W/m-KDIN 52612-1
Melting Point 260 °CISO 11357-1/-3
Maximum Service Temperature, Air 135 °Cfor 50% loss of tensile strength after 5000hr
 165 °Cfor 50% loss of tensile strength after 20000hr
 240 °C
Deflection Temperature at 0.46 MPa (66 psi) 250 °CISO 527-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 245 °CISO 527-1/-2
Decomposition Temperature >= 310 °C
Flammability, UL94 HB
@Thickness 1.60 mm
Ignition Temperature >= 400 °CASTM D1929
 
Processing PropertiesOriginal ValueComments
Processing Temperature 80.0 °CHopper Throat
Zone 1 290 °CFeed zone
Zone 2 290 °CCompression
Zone 3 290 °CMetering-zone
Zone 4 290 °CNozzle
Melt Temperature 280 - 300 °CInjection Molding/Extrusion
 290 °COptimal
Mold Temperature 80.0 °COptimal
 80.0 - 90.0 °CInjection Molding
Drying Temperature 80.0 °C
Dry Time 4 hour
Moisture Content 0.030 - 0.060 %Optimal
 <= 0.15 %
 
Descriptive Properties
Commercial StatusEurope
Peripheral Screw Speed< 0.3 m/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® B3EG7 BK 00564 35% Glass Filled PA6 (Dry)
BASF Ultramid® A3EG5 25% Glass Filled PA66 (Conditioned)
Ascend Performance Materials Vydyne® R525J NT0721 Nylon 66, 25% Glass Filled
A. Schulman Diamond DIAMALOY 310 GF10 PC/Polyester Alloy, Impact Modified
BASF Ultramid® B3EG7 35% Glass Filled PA6 (Dry)

PBASG0359 / 131992

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.