MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Proto3000 Copper C18150 Processed by DMSL
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Nonferrous Metal; Copper Alloy

Material Notes: Highlights:
  • Chromium Zirconium Copper (CuCr1Zr)
  • Excellent electrical and thermal conductivity
  • mechanical and material properties stable up to 700°F
  • Age Hardenable
Applications:
  • Excellent thermal and electrical conductivity
  • Conformal induction coils
  • Regeneratively cooled nozzles
  • Plastic mold components

Information provided by Proto3000

Key Words: Direct Metal Laser Sintering
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 80.080.0Z Axis, SR + Hot Isostatic Press (HIP)
 87.087.0Z Axis, SR + HIP + SHT + Precipitation Strengthening (PHT)
 90.090.0Z Axis, As Built
 94.094.0Z Axis, SR + HIP + Solution Anneal (SHT)
 108108Z Axis, Stress Relief (SR)
Tensile Strength, Ultimate 207 MPa30000 psiZ Axis, As Built
 239 MPa34600 psiZ Axis, Stress Relief (SR)
 250 MPa36300 psiZ Axis, SR + Hot Isostatic Press (HIP)
 255 MPa37000 psiZ Axis, SR + HIP + Solution Anneal (SHT)
 379 MPa55000 psiZ Axis, SR + HIP + SHT + Precipitation Strengthening (PHT)
Tensile Strength, Yield 110 MPa16000 psiZ Axis, SR + Hot Isostatic Press (HIP)
 117 MPa17000 psiZ Axis, SR + HIP + Solution Anneal (SHT)
 152 MPa22000 psiZ Axis, As Built
 186 MPa27000 psiZ Axis, Stress Relief (SR)
 248 MPa36000 psiZ Axis, SR + HIP + SHT + Precipitation Strengthening (PHT)
Elongation at Break 14.0 %14.0 %Z Axis, Stress Relief (SR)
 31.0 %31.0 %Z Axis, As Built
 31.0 %31.0 %Z Axis, SR + HIP + SHT + Precipitation Strengthening (PHT)
 47.0 %47.0 %Z Axis, SR + Hot Isostatic Press (HIP)
 48.0 %48.0 %Z Axis, SR + HIP + Solution Anneal (SHT)
Tensile Modulus 0.0960 GPa13.9 ksiZ Axis, Stress Relief (SR)
 0.103 GPa14.9 ksiZ Axis, As Built
 0.110 GPa16.0 ksiZ Axis, SR + HIP + Solution Anneal (SHT)
 0.117 GPa17.0 ksiZ Axis, SR + Hot Isostatic Press (HIP)
 0.124 GPa18.0 ksiZ Axis, SR + HIP + SHT + Precipitation Strengthening (PHT)
 
Component Elements PropertiesMetricEnglishComments
Chromium, Cr 0.500 - 1.50 %0.500 - 1.50 %
Nitrogen, N <= 0.100 %<= 0.100 %
Other, total <= 0.300 %<= 0.300 %
Oxygen, O <= 0.100 %<= 0.100 %
Zirconium, Zr 0.0500 - 0.200 %0.0500 - 0.200 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NPROTO805 / 322918

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.