MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pyrotek Pyrocast 220HT Refractory Castable
Categories: Ceramic; Carbide; Oxide; Silicon Oxide

Material Notes: Pyrocast 220HT is a high-performance refractory castable based on fused silica and silicon carbide.

Applications

  • Transfer troughs
  • Launder linings
  • Filter boxes
  • Pins and spouts

Advantages

  • Thermal shock resistance
  • High strength and erosion resistance
  • High service temperature
  • Non-wetting in continuous aluminum casting applications
  • Non-wetting to aluminum alloys that contain high levels of Mg, Zn and Si

Information provided by Pyrotek.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.115 g/cc
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.0100 GPa
@Treatment Temp. 725 °C
ASTM C133-84
Compressive Strength 50.0 MPacured at 725°C, based on ASTM C133-84
 
Thermal PropertiesOriginal ValueComments
CTE, linear 1.80 µm/m-°C
@Temperature 100 - 1000 °C
Thermal Conductivity 0.790 W/m-K
@Temperature 400 °C
 1.08 W/m-K
@Temperature 550 °C
 1.45 W/m-K
@Temperature 700 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 1100 °CRecommended for use in continuous casting applications

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Pyrotek Pyrocast AR Castable Refractory
Pyrotek Pyrocast AR PLUS Castable Refractory
Pyrotek PTB 2200 Structural Board
Pyrotek Pyrocast AR70 Low-Density Refractory Castable
Pyrotek Pyrocast AR-S Castable Refractory

CPYRO203 / 1920

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.