MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 6262-T651
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Data provided by Alcoa. General 6262 characteristics and uses: Good machinability and high strength; high corrosion resistance and applied coating acceptance. Finishing characteristics better than 2011, 2017, 2024, 7075 and equal to 6061. The T8 temper offers excellent residual stress control.

Uses: Camera parts, couplings, marine fittings, decorative and misc. hardware, hinge pins, knobs, magneto parts, nuts, oil line fittings, appliance fittings, roller skate parts, steam iron parts, TV fittings, tripod fittings, valves and valve parts.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96262; ISO AlMg1SiPb; AA6262-T651; Al6262-T651
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.72 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 290 MPa
 234 MPa
@Temperature 149 °C
 290 MPa
@Temperature 100 °C
 310 MPa
@Temperature 24.0 °C
 324 MPa
@Temperature -28.0 °C
 338 MPa
@Temperature -80.0 °C
 414 MPa
@Temperature -196 °C
Tensile Strength, Yield >= 241 MPa
 214 MPa
@Strain 0.2 %,
Temperature 149 °C
 262 MPa
@Strain 0.2 %,
Temperature 100 °C
 276 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 283 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 290 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 324 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 10 %in 5 cm.
 17 %
@Temperature -28.0 °C
 17 %
@Temperature 24.0 °C
 18 %
@Temperature -80.0 °C
 18 %
@Temperature 100 °C
 20 %
@Temperature 149 °C
 22 %
@Temperature -196 °C
Modulus of Elasticity 69.0 GPaAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Shear Modulus 26.0 GPaEstimated from similar Al alloys.
Shear Strength 175 MPaEstimated from ultimate tensile strength
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000390 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 25.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.890 J/g-°C
Thermal Conductivity 170 W/m-KEstimated from other heat treatments.
Melting Point 1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 1080 °FAA; Typical
Liquidus 1205 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 780 °Fhold at temperature 2 to 3 hr
Solution Temperature 1000 °Fhold at temperature 8 to 12 hr
Aging Temperature 340 °Fhold at temperature 8 to 12 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 94.6 - 97.8 %As remainder
Bismuth, Bi 0.40 - 0.70 %
Chromium, Cr 0.04 - 0.14 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Lead, Pb 0.40 - 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6262-T6
Aluminum 6262-T9
Aluminum 6262-T8
Alclad Aluminum 6061-T6, T651

MA6262T651 / 9486

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.