MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lotte Advanced Materials Infino® GC-1015 PC/ABS, FR  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: Eco-Friendly - 30% PCM

Information provided by Samsung Cheil Industries.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
ASTM D955
Melt Flow 25 g/10 min
@Load 10.0 kg,
Temperature 220 °C
25 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 116116ASTM D785
Tensile Strength at Break 63.7 MPa9240 psi50 mm/min; ASTM D638
Tensile Strength, Yield 60.8 MPa8820 psi50 mm/min; ASTM D638
Elongation at Break 102 %102 %50 mm/min; ASTM D638
Tensile Modulus 2.35 GPa341 ksi50 mm/min; ASTM D638
Flexural Strength 88.3 MPa12800 psi2.8 mm/min; ASTM D790
Flexural Modulus 2.45 GPa356 ksi2.8 mm/min; ASTM D790
Izod Impact, Notched  1.57 J/cm
@Thickness 6.35 mm
2.94 ft-lb/in
@Thickness 0.250 in
ASTM D256
 6.96 J/cm
@Thickness 3.17 mm
13.0 ft-lb/in
@Thickness 0.125 in
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 95.0 °C
@Thickness 6.40 mm
203 °F
@Thickness 0.252 in
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C
@Thickness 6.40 mm
176 °F
@Thickness 0.252 in
ASTM D648
Vicat Softening Point 98.0 °C208 °FB/50; ISO R306
 101 °C214 °FB/120; ISO R306
UL RTI, Electrical 95.0 °C203 °F
UL RTI, Mechanical with Impact 85.0 °C185 °F
UL RTI, Mechanical without Impact 90.0 °C194 °F
Flammability, UL94  V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 5VB
@Thickness 3.00 mm
5VB
@Thickness 0.118 in
 5VA
@Thickness 2.00 mm
5VA
@Thickness 0.0787 in

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Techmer ES Plastiblend® PC/ABS FR 1950 BK
Techmer ES Plastiblend® PC/ABS FR 6206 UV
Techmer ES Plastiblend® PC/ABS FR 6209
Techmer ES HiFill FR® ABS FR
Polymer Resources ABS-FR-[color]-UV Flame Retardant ABS, UV-stabilized

PSAMSU741 / 146558

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.