MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EN 1.0036 High Manganese Carbon Steel
Categories: Metal; Ferrous Metal; Carbon Steel; Low Carbon Steel

Key Words: EN 10025(90)A1(93) 1.0036. Similar to AISI 1513, UNS G15130
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/ccEstimated by MatWeb from similar grade
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 340 - 470 MPa
@Thickness 16.0 - 25.0 mm
Structural, Hot Rolled, Base Steel
 340 - 470 MPa
@Thickness 3.00 - 16.0 mm
Structural, Hot Rolled, Quality Steel
 360 - 510 MPa
@Thickness <=1.00 mm
Structural, Hot Rolled, Quality Steel
 360 - 510 MPa
@Thickness <=16.0 mm
Structural, Hot Rolled, Base Steel
Tensile Strength, Yield 235 MPa
@Thickness <=1.00 mm
Structural, Hot Rolled, Quality Steel
 235 MPa
@Thickness 16.0 - 25.0 mm
Structural, Hot Rolled, Base Steel
 235 MPa
@Thickness <=16.0 mm
Structural, Hot Rolled, Base Steel
 235 MPa
@Thickness 3.00 - 16.0 mm
Structural, Hot Rolled, Quality Steel
Elongation at Break 15 %
@Thickness <=1.00 mm
Transverse. Structural, Hot Rolled, Quality Steel
 15 %
@Thickness <=16.0 mm
Transverse. Structural, Hot Rolled, Base Steel
 15 %
@Thickness 3.00 - 16.0 mm
Transverse. Structural, Hot Rolled, Quality Steel
 17 %
@Thickness <=1.00 mm
Longitudinal. Structural, Hot Rolled, Quality Steel
 17 %
@Thickness <=16.0 mm
Longitudinal. Structural, Hot Rolled, Base Steel
 17 %
@Thickness 3.00 - 16.0 mm
Longitudinal. Structural, Hot Rolled, Quality Steel
 24 %
@Thickness 16.0 - 25.0 mm
Transverse. Structural, Hot Rolled, Base Steel
 26 %
@Thickness 16.0 - 25.0 mm
Longitudinal. Structural, Hot Rolled, Base Steel
Modulus of Elasticity 200 GPaEstimated by MatWeb from similar grade
Poissons Ratio 0.29Estimated by MatWeb from similar grade
Shear Modulus 80.0 GPaEstimated by MatWeb from similar grade
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000170 ohm-cmEstimated by MatWeb from similar grade
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°CEstimated by MatWeb from similar grade
Specific Heat Capacity 0.470 J/g-°CEstimated by MatWeb from similar grade
Thermal Conductivity 52.0 W/m-KEstimated by MatWeb from similar grade
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.17 %
Iron, Fe >= 98.3 %As Balance
Manganese, Mn <= 1.4 %
Nitrogen, N <= 0.0070 %N max na if Al >= 0.020
Phosphorus, P <= 0.045 %
Sulfur, S <= 0.045 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T4; 6061-T451
Aluminum 6061-O
EN 1.0037 High Manganese Carbon Steel, t < 16 mm
AISI 1513 Steel Composition Spec (UNS G15130)
AISI 1045 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round

M9ZE10036 / 232244

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.