MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Udel® GF-110 PSU, 10% glass fiber
Categories: Polymer; Thermoplastic; Polysulfone (PSU); Polysulfone, 10% Glass Fiber Reinforced

Material Notes: Udel® GF-110, resin is a 10% glass fiber reinforced polysulfone (PSU). Glass fiber substantially increases the rigidity, tensile strength, creep resistance, dimensional stability and chemical resistance of the polysulfone resin. The high performance properties and attractive price make these resins particularly effective alternatives to metals in many engineering applications.

- Natural: Udel® GF-110 NT

Applications: Appliance Components; Appliances; Connectors; Fittings; Food Service Applications; Industrial Parts; Microwave Cookware; Plumbing Parts; Valves/Valve Parts

Features: Acid Resistant; Alcohol Resistant; Alkali Resistant; Chemical Resistant; Creep Resistant; Good Dimensional Stability; Good Strength; High Heat Resistance; High Rigidity; Hydrocarbon Resistant; Hydrolytically Stable

Information provided by Solvay Specialty Polymers.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.33 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0040 cm/cmASTM D955
Melt Flow 6.5 g/10 min
@Load 2.16 kg,
Temperature 343 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 77.9 MPaASTM D638
Elongation at Break 4.0 %ASTM D638
Tensile Modulus 3720 MPaASTM D638
Flexural Strength 128 MPaASTM D790
Flexural Modulus 3790 MPaASTM D790
Izod Impact, Notched 48.0 J/mASTM D256
Tensile Impact Strength 101 kJ/m²ASTM D1822
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.00e+16 ohm-cmASTM D257
Dielectric Constant 3.15
@Frequency 1e+6 Hz
ASTM D150
 3.18
@Frequency 60 Hz
ASTM D150
Dielectric Strength 19.0 kV/mmASTM D149
Dissipation Factor 0.00070
@Frequency 60 Hz
ASTM D150
 0.0060
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 179 °CUnannealed; ASTM D648
Flammability, UL94 HB
@Thickness 3.20 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 343 - 399 °CInjection
Mold Temperature 121 - 163 °C
Drying Temperature 149 - 163 °C
Back Pressure 0.345 - 0.689 MPa
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorNatural Color; Opaque
FormsPellets
Injection RateFast
ProcessingExtrusion; Injection Molding
RoHS ComplianceYes
Screw Compression Ratio2.0:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4575 / 280375

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.