MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Avient Edgetek® PF-05GF/000 FR MR Polysulfone (PSU)
Categories: Polymer; Thermoplastic; Polysulfone (PSU)

Material Notes: The Edgetek® Engineering Thermoplastic Compounds portfolio covers a broad range of standard and custom-formulated high performance materials. This portfolio includes high-temperature materials for elevated service temperature environments, high-modulus / structural materials for load-bearing and high-strength applications and flame-retardant products. These compounds are based on select engineering thermoplastic resins that are compounded with reinforcing additives such as carbon fiber, glass fiber and glass beads.

Information provided by PolyOne

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.30 g/cc1.30 g/ccASTM D792
Filler Content 5.0 %5.0 %Glass Fiber Reinforcement
Water Absorption 0.50 %
@Thickness 3.18 mm
0.50 %
@Thickness 0.125 in
@ 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 68.9 MPa9990 psiType I, 5.1 mm/min; ASTM D638
Elongation at Break 10 %10 %Type I, 5.1 mm/min; ASTM D638
Tensile Modulus 3.10 GPa450 ksiType I, 5.1 mm/min; ASTM D638
Flexural Modulus 0.103 GPa14.9 ksiASTM D790
Izod Impact, Notched 0.590 J/cm
@Thickness 3.18 mm,
Temperature 23.0 °C
1.11 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 166 °C
@Thickness 3.18 mm
331 °F
@Thickness 0.125 in
Unannealed; ASTM D648
Flammability, UL94 V-0V-0UL 94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 343 - 382 °C649 - 720 °F
Mold Temperature 135 - 149 °C275 - 300 °F
Drying Temperature 135 - 149 °C275 - 300 °F
Dry Time 2.00 hour2.00 hour
 
Descriptive Properties
FormsPellets
Generic MaterialPSU
Generic NamePolysulfone (PSU)
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultrason® S 2010 PSU
Avient Edgetek® PF-20GF/000 Polysulfone (PSU)
Avient Edgetek® PF-1000 Polysulfone
BASF Ultrason® S 3010 PSU
Ensinger TECAPEI® 10% Glass Reinforced, made from Ultem® 2100 PEI

PH0POL0786 / 145355

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.