MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
Proto3000 ULTEM* 9085 Fused Deposition Modeling Polymer
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: Description: ULTEM* 9085 is a flame retardant high performance thermoplastic for direct digital manufacturing and rapid prototyping. It is ideal for the transportation industry due to its high strength-to-weight ratio and its V0 rating for FST (flame, smoke, and toxicity). This unique material’s preexisting certifications make it an excellent choice for the commercial transportation industry – especially aerospace, marine and ground vehicles. Combined with a Fortus 3D Production System, ULTEM 9085 allows design and manufacturing engineers to produce fully functional parts that are ideal for advanced functional prototypes or end use without the cost or lead time of traditional tooling.

Available Colors: Tan

Information provided by Proto3000 for their protoyping engineering services.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.34 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 71.64 MPaType 1, 2"/min; ASTM D638
Elongation at Break 5.9 %ASTM D790
Tensile Modulus 2220 MPaASTM D638
Flexural Strength 115.1 MPaMethod 1, 0.05"/min; ASTM D790
Flexural Modulus 2507 MPaASTM D790
Izod Impact, Notched 106 J/mMethod A; ASTM D256
Izod Impact, Unnotched 6.138 J/cmMethod A; ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 153 °CASTM D648
Glass Transition Temp, Tg 186 °CDAM (SSYS)
Oxygen Index 49 %ASTM D2863
 
Descriptive Properties
FAA Flammability<5FAR 25.853
OSU Peak Heat Release36 kW/m2FAR 25.853
OSU Total Heat Release66 kW.min/m2FAR 25.853
Vertical Burn2 secondstest at (60s), passes at, FAR 25.853

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Stratasys® Ultem 9085 for Rapid Prototyping
Quantum PEI - Ultem®
3D Systems Fused Deposition Modeling Material ULTEM
Quantum PEI - Ultem® 30% Glass Fiber Filled
Stratasys® PC Polycarbonate for 3D Printing

PPROTO975 / 133178

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.