MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Total LLDPE LL 1820 H Linear Low Density Polyethylene - Blown Film
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade

Material Notes: LL 1820 H is an ethylene-butene copolymer produced in a gas phase reactor. It is designed for delivering competitive performance in most blown film applications.

LL 1820 H can be processed at high output rates with moderate extrusion pressure, good bubble stability and gauge control on blown film machine designed for LLDPE.

LL 1820 H can advantageously be blended with LDPE or other PE resins used in blown film mono extrusion or coextrusion to improve film properties.

LL 1820 H is suited for many applications in the field of consumer, industrial, food or hygiene packaging such as collation shrink, liners, Form-Fill-Seal, heavy-duty sacks, refuse sacks or other bags and non-packaging applications like agriculture films e.g. tunnel and mulching films.

Contains antioxidant, slip agent and antiblock agent.

Information provided by Total Petrochemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.921 g/cc0.921 g/ccISO 1183
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
Antiblock Level 3200 ppm3200 ppm
Slip Level 1500 ppm1500 ppmErucamide
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 11.0 MPa1600 psiISO 527-3
Film Tensile Strength at Yield, TD 11.0 MPa1600 psiISO 527-3
Film Elongation at Break, MD 850 %850 %ISO 527-3
Film Elongation at Break, TD 900 %900 %ISO 527-3
Elmendorf Tear Strength, MD 5.60 g/micron142 g/milISO 6383-2
Elmendorf Tear Strength, TD 10.7 g/micron272 g/milISO 6383-2
Dart Drop Test 130 g0.287 lbISO 7765-1
Film Tensile Strength at Break, MD 35.0 MPa5080 psiISO 527-3
Film Tensile Strength at Break, TD 32.0 MPa4640 psiISO 527-3
1% Secant Modulus, MD 215 MPa31200 psiISO 178
1% Secant Modulus, TD 245 MPa35500 psiISO 178
 
Thermal PropertiesMetricEnglishComments
Melting Point 121 °C250 °FISO 11357
Vicat Softening Point 100 °C212 °FISO 306
 
Optical PropertiesMetricEnglishComments
Haze 14 %14 %ISO 14782
Gloss 54 %54 %at 45°; ASTM D2457
 
Processing PropertiesMetricEnglishComments
Processing Temperature 170 - 210 °C338 - 410 °FExtrusion Temp
Die Opening >= 0.180 cm>= 0.0709 in
Blow-up Ratio (BUR) 2.0 - 3.02.0 - 3.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil LLDPE LL 1002.80 Linear Low Density Polyethylene Resin
Total Lotrene® Q2018H Linear Low Density Polyethylene, Blown Film
ExxonMobil NTX™ NTX 141 Super Strength Film Resin
ExxonMobil NTX™ NTX 095 Super Strength Film Resin
ExxonMobil LDPE LD 306.75 Low Density Polyethylene Resin

PTOTAL738 / 130463

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.