MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Makrolon® 6267 Polycarbonate, Flame Retardant Grade  (discontinued **)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes:
  • ISO 7391-PC,MFLR,(,,)-18-9
  • Formerly Makrolon DP1-1872
  • MVR (300 °C/1.2 kg) 19 cm3/10 min
  • Flame retardant
  • UL 94V-0/1.5 mm
  • Low viscosity
  • UV stabilized
  • Easy release
  • Injection molding - Melt temperature 280 - 320 °C
  • Available in opaque colors only

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccISO 1183
Melt Density 1.02 g/cc
@Temperature 280 °C
Water Absorption 0.30 %Similar to ISO 62
Moisture Absorption at Equilibrium 0.12 %Similar to ISO 62
Linear Mold Shrinkage, Flow 0.0070 cm/cmISO 294-4,2577
Linear Mold Shrinkage, Transverse 0.0070 cm/cmISO 294-4,2577
Melt Flow 19 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 67.0 MPaISO 527-1/-2
Elongation at Break >= 50 %Nominal; ISO 527-1/-2
Elongation at Yield 6.0 %ISO 527-1/-2
Tensile Modulus 2450 MPaISO 527-1/-2
Charpy Impact Unnotched NBISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/1eU
Impact 5000Puncture - maximum force (N); ISO 6603-2
 5900
@Temperature -30.0 °C
Puncture - maximum force (N); ISO 6603-2
Puncture Energy 50.0 JISO 6603-2
 55.0 J
@Temperature -30.0 °C
ISO 6603-2
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mmIEC 60243-1
Dissipation Factor 0.00080
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 225 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 65.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 65.0 µm/m-°CISO 11359-1/-2
Specific Heat Capacity 1.70 J/g-°CMelt
Thermal Conductivity 0.173 W/m-KMelt
Deflection Temperature at 0.46 MPa (66 psi) 134 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 122 °CISO 75-1/-2
Vicat Softening Point 144 °C50°C/h 50N; ISO 306
Flammability, UL94 V-0
@Thickness 1.50 mm
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
IEC 60695-11-10
Oxygen Index 35 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 °CInjection Molding; ISO 294
 280 - 320 °C
Mold Temperature 80.0 °CInjection Molding; ISO 10724
 80.0 - 120 °C
 80.0 - 120 °C
Ejection Temperature 130 °C
Injection Velocity 200 mm/secISO 294
Drying Temperature 120 °C
Dry Time 2.00 - 3.00 hourDry air dryer
 2.00 - 4.00 hourFresh air dryer (high speed dryer)
 4.00 - 12.0 hourCirculating air drying oven (50 % fresh air)
Moisture Content <= 0.020 %
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 India
 Near East/Africa
 North America
 South and Central America
Eff. thermal diffusivity (m²/s)1E-07
FeatureLight stabilized or stable to light
 Release agent
 U.V. stabilized or stable to weather
FormPellets
ProcessInjection Molding
UL recognitionUL\l1.5\n
 UL\lh\n

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Makrolon® 6265 Polycarbonate, Flame Retardant Grade
Covestro Bayblend® FR3010 HF PC/ABS Blend
Covestro Makrolon® 6267X Polycarbonate
Covestro Makrolon® 2865 Polycarbonate, Flame Retardant Grade
Covestro Makrolon® 2467 Polycarbonate

PB09926 / 92766

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.