MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex TELCAR® TELC 1000-92UV BLACK 550 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Notes: Telcar TELC 1000-92 UV-2 BLACK 550 is a high hardness, low density high performance thermoplastic elastomer designed for various applications in the automotive and consumer/industrial segments. Telcar TELC 1000-92 UV-2 BLACK 550 has good UV resistance, good impact resistance and is suitable for injection molding.

Features: Chemical Resistant; Good Adhesion; Good Impact Resistance; Good Processability; High Hardness; Low Density; UV Resistant

Uses: Automotive Exterior Parts; Automotive Interior Parts; Industrial Applications; Rubber Replacement

Automotive Specifications: CHRYSLER MS-DB-590 CPN4844 Color: Black

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.913 g/ccASTM D792
Viscosity 516 cP
@Temperature 200 °C
Apparent, 206 sec-1; ASTM D3795
Linear Mold Shrinkage 0.011 cm/cmFlow, 24 hours; ASTM D955
 0.013 cm/cmFlow, After 30 min. at 180°F; ASTM D955
Melt Flow 2.6 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 43.7
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
ISO 188
Hardness, Shore D 42
@Time 10.0 sec
ASTM D2240
 49
@Time 1.00 sec
ISO 868
 49
@Time 1.00 sec
ISO 868
Tensile Strength at Break 9.93 MPaFlow; ISO 37
 1070 psiAcross Flow; ISO 37
 4.21 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow; ISO 188
 4.43 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
Flow; ISO 188
 5.66 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow; ISO 188
 5.96 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
Flow; ISO 188
Tensile Stress at Strain 1020 psi
@Strain 100 %
Across Flow; ISO 37
 1390 psi
@Strain 100 %
Flow; ISO 37
Elongation at Break 270.0 %Flow; ISO 37
 370 %Across Flow; ISO 37
 89.1 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow; ASTM D573
 99.9 %
@Treatment Temp. 116 °C,
Time 3.629e+6 sec
Flow; ASTM D573
 122.1 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow; ASTM D573
 136.9 %
@Treatment Temp. 121 °C,
Time 3.629e+6 sec
Across Flow; ASTM D573
Flexural Modulus 42100 psiASTM D790
Izod Impact, Notched NB
@Temperature -40.0 °C
ASTM D256
Gardner Impact 300 in-lb
@Temperature -22.0 °C
ASTM D3029
Tensile Impact Strength 224 ft-lb/in²ASTM D1822
Dart Drop, Total Energy 200 ft-lb
@Temperature -40.0 °C
@ Yield, 9000 in/min, Ductile Failure
 350 ft-lb
@Temperature -40.0 °C
@ Break, 9000 in/min, Ductile Failure
Tear Strength 364 pliDie C; ASTM D1004
 500 pliAcross Flow; ISO 34-1
Compression Set 60 %
@Temperature 22.8 °C,
Time 79200 sec
ISO 815
 74 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 93 %
@Temperature 90.0 °C,
Time 252000 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
CTE, linear 119 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM D696
CTE, linear, Transverse to Flow 117 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 62.5 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 40.7 °CASTM D648
Glass Transition Temp, Tg -55.9 °CASTM E1356
Flame Spread 30.2 in/minPass: Burn Rate- Max 100; FMVSS 302
 
Descriptive Properties
Fogging92, 3 hours at 100°C, Haake buchler

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, No Plasticizer
Seals Eastern 5433 Nitrile Rubber
Network Polymers Softflex® 0150
Multibase Multi-Flex® TPE D 4308 BLK
Kuraray SEPTON® S1001 Thermoplastic Rubber

PTEKNO307 / 70050

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.