MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter Micro-Melt® 10 Tough Treated Tool Steel (AISI A11)
Categories: Metal; Ferrous Metal; Tool Steel

Material Notes: Micro-Melt® 10 tool steel is a high vanadium tool steel produced using the Carpenter Micro-Melt powder process. This grade possesses wear resistance superior to most other tool steels along with good strength and toughness characteristics. Many of the benefits realized in the use of Micro-Melt powder metals, such as Micro-Melt® 10 alloy, are a direct result of the refined microstructure (smaller, more uniformly distributed carbide particles and a finer grain size) and the lack of segregation in the powder metallurgy product. These advantages include ease of grinding, improved response to heat treatment, greater wear resistance, and increased toughness of the finished tool. Micro-Melt 10 tool steel changes size only slightly after hardening. An expansion of about 0.0004 inches/inch is typical.

Applications: punches, dies for blanking, piercing dies, forming rolls and dies, cold heading, steel mill rolls, cold extrusion, slitter knives, shears, pelletizer blades, nozzles, woodworking tools, cold extrusion barrels, cold extrusion liners, plastic injection molds, compacting tools

Information provided by Carpenter Technology Corporation.

Micro-Melt® is a registered trademark of Carpenter Technology Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 7.45 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 59
Tensile Strength at Break 5171 MPa
Tensile Strength, Ultimate 5205 MPa
Modulus of Elasticity 200 GPa
Izod Impact Unnotched 39.3 J
Abrasion 12loss in mm3, after 30 minutes; ASTM G65
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.72 µm/m-°C
@Temperature 21.0 - 100 °C
 11.13 µm/m-°C
@Temperature 21.0 - 260 °C
 12.32 µm/m-°C
@Temperature 21.0 - 538 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 2.4 - 2.5 %
Chromium, Cr 4.75 - 5.75 %
Iron, Fe 78.21 - 81.35 %As Balance
Manganese, Mn 0.35 - 0.60 %
Molybdenum, Mo 1.1 - 1.5 %
Silicon, Si 0.75 - 1.1 %
Sulfur, S 0.050 - 0.090 %
Vanadium, V 9.25 - 10.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Carpenter Micro-Melt® 10 Hardened and Tempered Tool Steel (AISI A11)
Carpenter Micro-Melt® 10 Wear Treated Tool Steel (AISI A11)
Crucible Steel CPM® 10V® (AISI A11) Tool Steel
Bohler-Uddeholm BÖHLER K294 MICROCLEAN AISI A11 Powder Metal Tool Steel
Carpenter Micro-Melt® 9 Tough Treated Tool Steel

NCARN06 / 15845

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.