MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2024-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: General 2024 characteristics and uses (from Alcoa): Good machinability and surface finish capabilities. A high strength material of adequate workability. Has largely superseded 2017 for structural applications. Use of 2024-O not recommended unless subsequently heat treated.

Uses: Aircraft fittings, gears and shafts, bolts, clock parts, computer parts, couplings, fuse parts, hydraulic valve bodies, missile parts, munitions, nuts, pistons, rectifier parts, worm gears, fastening devices, veterinary and orthopedic equipment, structures.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
A Zr + Ti limit of 0.20 percent maximum may be used with this alloy designation for extruded and forged products only, but only when the supplier and the purchaser have mutually agreed.
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 2024-O; UNS A92024; ISO AlCu4Mg1; NF A-U4G1 (France); DIN AlCuMg2; AA2024-O, ASME SB211; CSA CG42 (Canada); Al2024-O
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.78 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 47AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 27.0 ksiAA; Typical
 <= 220 MPaSheet and plate
 <= 220 MPaDrawn tube
 <= 240 MPaWire, rod, and bar (rolled or cold finished)
 <= 240 MPaWire, rod, bar and shapes (extruded)
 <= 240 MPaExtruded tube
 <= 240 MPaRivet and cold-heading wire and rod
Tensile Strength, Yield 11.0 ksiAA; Typical
 <= 95.0 MPaSheet and plate
 <= 105 MPaDrawn tube
 <= 130 MPaWire, rod, bar and shapes (extruded)
 <= 130 MPaExtruded tube
Elongation at Break >= 12 %Sheet and plate
 >= 12 %Wire, rod, bar and shapes (extruded)
 >= 12 %Extruded tube
 >= 16 %Wire, rod, and bar (rolled or cold finished)
 20 %
@Thickness 1.59 mm
AA; Typical
 22 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Ultimate Bearing Strength 345 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 131 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33
Fatigue Strength 13000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 30 %0-100 Scale of Aluminum Alloys
Shear Modulus 28.0 GPa
Shear Strength 18.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 21.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.9 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 21.1 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.9 µm/m-°C
@Temperature 20.0 - 100 °C
 23.8 µm/m-°C
@Temperature 20.0 - 200 °C
 24.7 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.875 J/g-°C
Thermal Conductivity 1340 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 935 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 935 °FAA; Typical
Liquidus 1180 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 493 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.7 - 94.7 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu 3.8 - 4.9 %
Iron, Fe <= 0.50 %
Magnesium, Mg 1.2 - 1.8 %
Manganese, Mn 0.30 - 0.90 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.50 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2024-T3
Aluminum 2024-T6
Aluminum 2024-T4; 2024-T351
Aluminum 6061-O
Aluminum 2024-T361

MA2024O / 8864

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.