MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Novamid® 3010GN30 NAT PA66-GF30 FR(17)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: 30% Glass Reinforced, Flame Retardant

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.40 g/ccdry; ISO 1183
Moisture Absorption 1.60 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.0030 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.012 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 120 MPacond; ISO 527-1/-2
 170 MPadry; ISO 527-1/-2
Elongation at Break 2.0 %dry; ISO 527-1/-2
 2.9 %cond; ISO 527-1/-2
Tensile Modulus 8.00 GPacond; ISO 527-1/-2
 11.5 GPadry; ISO 527-1/-2
Flexural Strength 210 MPacond; ISO 178
 260 MPadry; ISO 178
Flexural Modulus 8100 MPacond; ISO 178
 10400 MPadry; ISO 178
Charpy Impact Unnotched 68.0 kJ/m²
@Temperature 23.0 °C
dry; ISO 179/1eU
 70.0 kJ/m²
@Temperature 23.0 °C
cond; ISO 179/1eU
Charpy Impact, Notched 11.0 kJ/m²
@Temperature 23.0 °C
dry; ISO 179/1eA
 14.0 kJ/m²
@Temperature 23.0 °C
cond; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 3.00e+14 ohm-cmdry; IEC 60093
Surface Resistance 4.00e+14 ohmcond; IEC 60093
Dielectric Constant 4.0
@Frequency 100 Hz
dry; IEC 60250
 4.0
@Frequency 1e+6 Hz
dry; IEC 60250
Dielectric Strength 23.0 kV/mmdry; IEC 60243-1
Dissipation Factor 0.0090
@Frequency 100 Hz
dry; IEC 60250
 0.019
@Frequency 1e+6 Hz
dry; IEC 60250
Comparative Tracking Index 175 Vdry; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 20.0 µm/m-°Cdry; ISO 11359-1/-2
CTE, linear, Transverse to Flow 60.0 µm/m-°Cdry; ISO 11359-1/-2
Melting Point 260 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 243 °Cdry; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 258 °Cdry; ISO 75-1/-2
Flammability, UL94 V-0
@Thickness 0.800 mm
dry; IEC 60695-11-10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Novamid® 3021GH30 NAT PA66-GF30
Envalior Akulon® SG-KGS6 PA66-GF30 FR
Envalior Novamid® 3021GH30 BK629 PA66-GF30
Envalior Akulon® S223-HG6 PA66-GF30, Dry, 30% Glass Filled, Heat Stabilized
Envalior Akulon® S223-HG6 PA66-GF30, Conditioned, 30% Glass Filled, Heat Stabilized

PDSM9840 / 161461

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.