MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Akro-Plastic Akromid® B3 2 RM-D black (3254) PA 6 Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Description: AKROMID B3 2 RM-D black (3254) is a nonreinforced, UV-stabilized polyamide 6 with limited moisture absorption. Applications are interior and exterior parts with improved impact strength in the automotive industry

Additive: UV Stabilizer

Features:

  • Good Impact Resistance
  • Low Moisture Absorption
Uses:
  • Automotive Applications
  • Automotive Exterior Parts
  • Automotive Interiors

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.10 g/ccISO 1183
Moisture Absorption 1.65 %
@Temperature 70.0 °C
Humidity, 62% RH; ISO 1110
Linear Mold Shrinkage, Flow 0.0080 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cmISO 294-4
Melt Flow 30 g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1183
Spiral Flow 65.0 cmCross section: 7 mm x 3.5 mm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 60.0 MPa50 [mm/min]; ISO 527-2
Elongation at Break >= 30 %50 [mm/min]; ISO 527-2
Tensile Modulus 2500 MPa1 [mm/min]; ISO 527-2
Flexural Modulus 2300 MPa2 [mm/min]; ISO 178
Charpy Impact Unnotched NB
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 10.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 15.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 225 °CDIN EN 11357-1
Deflection Temperature at 0.46 MPa (66 psi) 100 °CUnannealed; ISO 75/B
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °CUnannealed; ISO 75/A
Flammability, UL94 HB
@Thickness 0.800 mm
 
Processing PropertiesOriginal ValueComments
Feed Temperature 60.0 - 80.0 °C
Nozzle Temperature 240 - 280 °C
Zone 1 225 - 300 °C
Zone 2 225 - 300 °C
Zone 3 225 - 300 °C
Zone 4 225 - 300 °C
Melt Temperature 260 - 300 °C
Mold Temperature 80.0 - 100 °C
Drying Temperature 80.0 °C
Dry Time 4.00 - 12.0 hour
Hold Pressure 75.0 MPa
Back Pressure 5.00 - 10.0 MPa
 
Descriptive Properties
Resistance to AcetaldehydeFail100% Conc.
Resistance to Boric acidPass10% Conc
Resistance to Brake fluid (DOT 4)Pass10% Conc
Resistance to Dichloro-Acetic acidPass96% Conc
Resistance to Fruit JuicesPass50°C, 100% Conc
Resistance to Hydrogen chloride, gasPass100% Conc
Resistance to Iso-octanolPass100% Conc
Resistance to Oleic acidPass20% Conc
Resistance to Potassium permanganate, aqueousPass1% Conc
Resistance to SpiritsPass100% Conc
Resistance to TolueneFail100% Conc
Resistant to Citric acidPass10% Conc
Resistant to Hydrogen peroxideFail
Resistant to Sulfuric acidFail96% Conc
Resistant to WaterPass<50°C, 100% Conc
Resistant to Zinc chloride, aqueousPass50% Conc

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® B3 2 RM-D (3374) PA 6 Dry
Akro-Plastic Akromid® B3 2 RM-D (3374) PA 6 Conditioned
A. Schulman SCHULAMID® 6 MV5 Unreinforced Nylon 6
A. Schulman SCHULAMID® 6 MV14 Unreinforced Nylon 6
Azoty Tarnow™ Tarnamid® T-30 Polyamide 6 - Natural

PAKRO241 / 182828

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.