MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Daelim H&L Plavis-ESD CM Polyimide Bearing
Categories: Polymer; Thermoset; Polyimide, TS

Material Notes: Compression Molded. Plavis-ESD: Electrostatic dissipative, Electrostatic dissipative, high thermal resistance and superior mechanical properties. And surface resistivity 10²-10³ Ohm

General Plavis information for all grades:

PLAVIS polyimide has nitrogen bonded to 3 carbons is the critical part of the chain and imparts the plastic with remarkable features and benefits. PLAVIS is available as raw material or as molded parts, plates, and rods. PLAVIS isostatic molded rods have uniform properties in all directions.

Properties:

  • One of the highest temperature plastics in the world with a continuous operating temperature of 300°C. Well suited for cryogenic conditions
  • Retains high tensile strength and modulus even at high temperatures. Will not crack or creep under load.
  • Lowest out-gassing of any plastic at 300°C. Will not contaminate vacuum chamber process or products.
  • Grades are available for use at 1 million psi-fpm PV limit with lubrication, 300,000 psi-fpm PV limit without lubrication. Stable friction level.
  • Filled grades resistivity is tailorable.
  • Machines like brass-tiny and intricate features can be produced without cracking. Can be lapped to mirror finish.
Applications:
  • Flat Panel Display/Solar Cells:: Drying oven (HP/CP, Baking, IR) Glass support pins, Glass holders, Rollers; Cleaning EUV roller, Bearing; PVD/CVD Insulation parts Insert, Clamp, Bush, Caps, Susceptor pin, Ball bearing etc.; Etcher Screw, bolts. and Others Probe unit, station parts
  • Semiconductor: Wafer Processing Wafer clamp rings, Insulators, Screw & Fasteners, Vacuum pads, Alignment pins; Wafer handling, guides, and carriers, Vacuum pick up strips; IC handling & testing Die pick up collects, Test socket insulator
  • General Industry: Hot runner system Seal caps, Insulators; Plasma cutting torches parts Swirl rings, Insulator, Caps.; Heat resistance materials Bottle grippers, Conveyor tips; Scientific consumable parts GC/Mass ferrules, HPLC valve rotors; Textile Machines Valve seat, Bearing, Shedder Bushing
  • Automotive / Transportation:Transmissions Thrust Washers, Seal Rings, Valve Seats, Transmission Valve Balls, Check Valves; Electrical Motors Bushings, Washers, Thrust Plugs; Brakes Wear Pads, Valve Seats and Balls in ABS Systems; Fuel Systems Bushings, Seal Rings, Band Springs, Valve Seats; Turbo Chargers Ball Bearing Retainers, Wastegate Bushings; Vacuum Pump Vanes, Engine Belt Tensioners, Rubbing Blocks, Door Hinge Bushings, Gear Stick Rollers, Ignition Distributors, Constant Friction Pads for Split-Flywheels
  • Aerospace/Aircraft: Compressor Variable Vane Bushings and Washers, Aircraft Fan Thrust Reverser, Fan Blade Wear Strips, Locking Insert Nut, Fuel Line Spacer, Reciprocating Shaft Seal for Jet Engine Afterbunner Actuating System

Information provided by Daelim H&L

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.44 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 90 - 105ASTM D792
Tensile Strength, Ultimate 68.6 MPaASTM D1708
 39.2 MPa
@Temperature 260 °C
ASTM D1708
Elongation at Break 5.5 %ASTM D1708
 5.0 %
@Temperature 260 °C
ASTM D1708
Flexural Strength 107.9 MPaASTM D790
Flexural Modulus 3.432 GPaASTM D790
Compressive Strength 24.5 MPa
@Strain 1 %
ASTM D695
 147.1 MPa
@Strain 10 %
ASTM D695
Compressive Modulus 2452 MPaASTM D695
Izod Impact, Notched 5.00 kg-cm/cmASTM D256
Coefficient of Friction, Dynamic 0.32PV=10 kg/cm² · m/sec (0.98 MPa·m/sec)
 
Electrical PropertiesOriginal ValueComments
Surface Resistance 1.00e+6 - 1.00e+9 ohmASTM D257
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.370 W/m-K
Maximum Service Temperature, Air 300 °CContinuous
Deflection Temperature at 1.8 MPa (264 psi) 360 °C
Flammability, UL94 V-0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Daelim H&L Plavis-ESD DF Polyimide Bearing
Manganese Bronze, UNS C86200, Copper Casting Alloy
MetalTek C86300 High Tensile Manganese Bronze
MetalTek MTEK 65 UNS C90700 Gear Bronze
Manganese Bronze, UNS C86300, Copper Casting Alloy

PDAEL914 / 178361

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.