MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 890 RTM Resin - Woven Carbon Fabric Composite
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: CYCOM® 890 RTM is a one-part liquid epoxy resin system. It has one month out-life at room temperature which reduces the time required for the freeze-thaw-storage processes in a production environment. Its frozen storage shelf-life is 12 months at -18°C (0°F). CYCOM 890 RTM’s viscosity is low enough at 80°C (175°F) to allow injection without excessive heating of either the resin or the transfer pipework. When the resin is heated to cure temperature its viscosity is further reduced, helping to ensure full wet-out of the reinforcing fibers. CYCOM 890 RTM is fully cured after two hours at 180°C (355°F) after which it will have a continuous dry service performance of 170°C (338°F) and a continuous hot/wet service performance of 160°C (320°F) If needed, an optional free-standing postcure for two hours at 200°C (390°F) can be used. After postcure the resin will have a continuous dry service performance of 195°C (383°F) and a continuous hot/wet service performance of 170°C (338°F). CYCOM 890 RTM is compatible with the range of reinforcing fibers used in manufacturing composite components, i.e., carbon, glass, aramid, etc. A fully compatible binder system, CYCOM® 7720 has been developed for use with CYCOM 890 RTM. The binder is available pre-coated onto fabric. A separate datasheet for CYCOM 7720 is available on request.

Features & Benefits:

  • One-part system
  • 30 day out-life at room temperature
  • 12 month shelf-life at -18°C (0°F)
  • Injectable at 80°C (175°F) with a 24-hour pot-life
  • 250 cps initial injection viscosity
  • Less than 10 cps minimum viscosity
  • Two hours at 180°C (355°F) cure
  • 170°C (350°F) continuous dry service performance [195°C (383°F) after optional post-cure]
  • 160°C (320°F) continuous hot/wet service performance [170°C (338°F) after optional post-cure]
  • Fully compatible with CYCOM 7720 binder coating and CYCOM® 890-1 low resin content (LRC) filmfor tack enhancing fabrics
  • Low reactivity; No special shipping requirements
Applications: Infusion applications requiring low viscosity and extended pot-life
  • Control surfaces
  • Nacelle casing
  • Large surface fairings
  • Hinges/brackets/fittings
Mechanical property data for epoxy with 57% fiber volume T650 6K-5HS woven carbon fabric. 'Wet' property data after equilibration at 160 °F (70C) and 85% RH.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.22 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 49900 psi
@Temperature -55.0 °C
Open Hole
 51100 psi
@Temperature 24.0 °C
Open Hole
 53400 psi
@Temperature 82.0 °C
Open Hole, wet
 82700 psi
@Temperature -55.0 °C
Un-Notched
 87500 psi
@Temperature 24.0 °C
Un-Notched
 89800 psi
@Temperature 82.0 °C
Un-Notched, wet
 109500 psi
@Temperature -55.0 °C
Weft; SACMA SRM-4
 116300 psi
@Temperature 24.0 °C
Weft; SACMA SRM-4
 125600 psi
@Temperature 24.0 °C
Warp; SACMA SRM-4
 126600 psi
@Temperature 82.0 °C
Weft, wet; SACMA SRM-4
Tensile Modulus 71.8 GPaWarp; ASTM D638
 66.7 GPa
@Temperature 24.0 °C
Weft; ASTM D638
 66.8 GPa
@Temperature -55.0 °C
Weft; ASTM D638
 70.4 GPa
@Temperature 82.0 °C
Weft, Wet; ASTM D638
Flexural Strength 128600 psiWeft; ASTM D790
Flexural Modulus 51.2 GPa
@Temperature 24.0 °C
Weft; ASTM D790
Compressive Strength 190.7 MPa
@Temperature 82.0 °C
After impact, Wet
 225.7 MPa
@Temperature 82.0 °C
Open Hole, Wet
 226.6 MPa
@Temperature 24.0 °C
After impact
 246 MPa
@Temperature -55.0 °C
After impact
 268.1 MPa
@Temperature 24.0 °C
Open Hole
 306.5 MPa
@Temperature -55.0 °C
Open Hole
 349.2 MPa
@Temperature 82.0 °C
Un-Notched, Wet
 417.1 MPa
@Temperature 24.0 °C
Un-Notched
 458.1 MPa
@Temperature -55.0 °C
Un-Notched
 652.7 MPa
@Temperature 82.0 °C
Weft, Wet; SACMA SRM-1
 663.4 MPa
@Temperature 24.0 °C
Warp; SACMA SRM-1
 702.3 MPa
@Temperature 24.0 °C
Weft; SACMA SRM-1
 720 MPa
@Temperature -55.0 °C
Weft; SACMA SRM-1
Compressive Modulus 58900 MPa
@Temperature 24.0 °C
Weft; SACMA SRM-1
 59900 MPa
@Temperature -55.0 °C
Weft; SACMA SRM-1
 60400 MPa
@Temperature 82.0 °C
Weft, Wet; SACMA SRM-1
 63500 MPa
@Temperature 24.0 °C
Warp; SACMA SRM-1
Shear Modulus 4.80 GPaIn-plane
 3.80 GPa
@Temperature 82.0 °C
In-plane, Wet
 4.20 GPa
@Temperature 24.0 °C
In-plane
 4.80 GPa
@Temperature -55.0 °C
In-plane
Shear Strength 10100 psi
@Temperature 24.0 °C
Weft
 10400 psi
@Temperature 24.0 °C
Warp
 13700 psi
@Temperature 82.0 °C
In-plane, Wet
 16000 psi
@Temperature 24.0 °C
In-plane
 16800 psi
@Temperature -55.0 °C
In-plane
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 170 °Cwet
 195 °Cdry
Glass Transition Temp, Tg 169 °CE' onset, 48 hr water boil
 191 °CE' onset
 210 °Cpeak tan delta
 210 °Cpeak tan delta, wet, 48 hr water boil
 
Processing PropertiesOriginal ValueComments
Processing Temperature 355 °F
@Time 7200 sec
Cure
Shelf Life 12.0 Month
@Temperature -17.8 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with IM7-6K-4HS Fabric
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with T650-35-3K-PW Fabric
Solvay CYCOM® 5320-1 Epoxy with T40/800B Unidirectional Tape Composite
Solvay CYCOM® 977-3 Epoxy - Unidirectional Carbon Fiber Tape
Solvay CYCOM® 977-2 Epoxy - Carbon Fiber Laminate

PCYTED087a / 234743

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.