MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SCG Chemicals EL-Pro™ P722JO Polypropylene Injection Molding
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Key Characteristics:
  • Good flowability
  • Good sealability
  • Good mechanical property balance
  • Minimal shrinkage and warpage
  • Contains UV stabilizer

Recommended Applications:

  • Good impact automotive and electrical appliance parts
  • Battery case that require excellent properties

Information provided by SCG Chemicals

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.910 g/cc0.910 g/ccASTM D1505
Linear Mold Shrinkage, Flow 0.0152 cm/cm
@Thickness 2.00 mm
0.0152 in/in
@Thickness 0.0787 in
TPE Method
Linear Mold Shrinkage, Transverse 0.014 cm/cm
@Thickness 2.00 mm
0.014 in/in
@Thickness 0.0787 in
TPE Method
Melt Flow 10 g/10 min
@Load 2.16 kg,
Temperature 230 °C
10 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 7575ASTM D785
Tensile Strength at Break 18.0 MPa2610 psiASTM D638
Tensile Strength, Yield 29.4 MPa4270 psiASTM D638
Elongation at Break 200 %200 %ASTM D638
Flexural Modulus 1.27 GPa185 ksiASTM D790
Izod Impact, Notched  0.490 J/cm
@Temperature -20.0 °C
0.918 ft-lb/in
@Temperature -4.00 °F
ASTM D256
 0.686 J/cm
@Temperature 0.000 °C
1.29 ft-lb/in
@Temperature 32.0 °F
ASTM D256
 0.981 J/cm
@Temperature 23.0 °C
1.84 ft-lb/in
@Temperature 73.4 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 163 °C325 °FASTM D2117
Deflection Temperature at 0.46 MPa (66 psi) 110 °C230 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C131 °FASTM D648
Vicat Softening Point 150 °C302 °FASTM D1525
Brittleness Temperature -20.0 °C-4.00 °FASTM D746
 
Optical PropertiesMetricEnglishComments
Haze 80 %
@Thickness 1.00 mm
80 %
@Thickness 0.0394 in
ASTM D1003
Gloss 30 %
@Thickness 1.00 mm
30 %
@Thickness 0.0394 in
ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SCG Chemicals EL-Pro™ P642J Polypropylene Injection Molding
Aurora Plastics GPP1001V0M-HCO PP
Avient Maxxam™ FR PP 301 EXT Polypropylene
Bamberger Polymers Bapolene® 4072 Polypropylene, Injection Grade
ExxonMobil PP7033N Impact Copolymer

PSCGC958 / 120712

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.