MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SCG Chemicals EL-Lene™ H1000PC High Density Polyethylene Pipe Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Pipe Grade

Material Notes: Key Characteristics: Good processing, high thermal stability, low sagging, good balance of MRS, SCG, and RCP

Recommended Applications: Water pressure and gas pipes

Certification: Certified by EXOVA, LNE, AENOR, INSTA, GOST, PE100+ association

Information provided by SCG Chemicals

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.959 g/cc0.959 g/ccISO 1183
Environmental Stress Crack Resistance >= 10000 hour>= 10000 hourF0; ASTM D1693
Oxidative Induction Time (OIT) >= 70 min
@Temperature 200 °C
>= 70 min
@Temperature 392 °F
ISO/TR10837
Carbon Black Loading 2.3 %2.3 %ISO 6964
Melt Flow 0.25 g/10 min
@Load 5.00 kg,
Temperature 190 °C
0.25 g/10 min
@Load 11.0 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6464ASTM D2240
Tensile Strength at Break 35.0 MPa5080 psiCrosshead speed 100 mm/min; ISO 527
Tensile Strength, Yield 23.0 MPa3340 psiCrosshead speed 100 mm/min; ISO 527
Elongation at Break 791 %791 %Crosshead speed 100 mm/min; ISO 527
Flexural Modulus 1.00 GPa145 ksiASTM D790
Izod Impact, Notched  2.45 J/cm
@Temperature -20.0 °C
4.59 ft-lb/in
@Temperature -4.00 °F
ASTM D256
 3.14 J/cm
@Temperature 0.000 °C
5.88 ft-lb/in
@Temperature 32.0 °F
ASTM D256
 3.53 J/cm
@Temperature 23.0 °C
6.61 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Hydrostatic Design Basis 10.0 MPa1450 psiISO 9080
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature <= -60.0 °C<= -76.0 °FASTM D746
 
Descriptive Properties
Carbon Black/Pigment Dispersion (grade)<3ISO 18553
ColorBlack
Rapid Crack Propagation=12 barISO 13477
Resistance to Gas Constituents>20 hoursISO 1167
Resistance to Slow Crack Growth>500 hoursISO 13479

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Borealis BorSafe™ HE3494-LS-H HDPE Compound for Pressure Pipes
Ineos TUB 121NTW HDPE
Overview of materials for High Density Polyethylene (HDPE), Carbon Black Filled
SCG Chemicals EL-Lene™ H1000PBL High Density Polyethylene Pipe Resin
Chevron Phillips Marlex® HP076 High Density Polyethylene, Pipe Grade

PSCGC916 / 120670

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.