MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter Micro-Melt® M-3 Class 2 Alloy (AISI M3)
Categories: Metal; Ferrous Metal; Tool Steel

Material Notes: Micro-Melt® M-3 Class 2 alloy is a powder metal tungsten-molybdenum high-speed steel possessing the superior wear resistance characteristics required for difficult cutting operations. The advantages of Micro-Melt premium powder high speed steels include ease of grinding, response to heat treatment, more uniform structure, greater wear resistance and improved toughness. In addition, Carpenter's unique hot rolling and rotary forging capabilities impart minimal distortion characteristics to these alloys.

Applications: Broaches, Form tools, Drills, Counterbores, Milling cutters, End mills, Chasers, Taps, Lathe tools, Planer tools, Reamers

Information provided by Carpenter Technology Corporation.

Micro-Melt® is a registered trademark of Carpenter Technology Corporation.

Key Words: UNS T11323
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 8.16 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 57 - 59Tempered at 1150°F
 65 - 66As quenched
Modulus of Elasticity 207 GPa
Izod Impact Unnotched 32.5 - 42.0 J
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 1.25 %
Chromium, Cr 4.0 %
Iron, Fe 79.43 %As Balance
Molybdenum, Mo 6.0 %
Sulfur, S 0.070 %
Tungsten, W 6.25 %
Vanadium, V 3.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type M2 Molybdenum High Speed Tool Steel (UNS T11302)
Bohler-Uddeholm UDDEHOLM VANADIS 23 (AISI M3:2) Hot Work Tool Steel
AISI Type M3 Class 1 Molybdenum High Speed Tool Steel (UNS T11313)
Bohler-Uddeholm BÖHLER S601 (M2 Modified) High Speed Steel For Cold Work Applications
Carpenter Micro-Melt® M-4 Alloy (AISI M4)

NCARN11 / 15850

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.