MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Outokumpu 153MA™ High Temperature Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Variant of 1.4301 with increased silicon and nitrogen contents and microalloyed with rare earth metals (REM). This raises the max service temperature in dry air to 1000°C.

Applications: Heat and creep resistance. For use over 550°C for equipment and components within:

  • Iron, steel, and non-ferrous industries
  • Engineering industry
  • Energy conservation plants
  • Cement industry

Available in hot rolled plate (Quarto), cold rolled strip/sheet, cold rolled narrow strip, bar, and rod forms.

Key Words: EN 1.4818; UNS S30415
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/ccRT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 660 MPaOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 300 MPa
@Temperature 700 °C
EN min.
 385 MPa
@Temperature 600 °C
EN min.; EN 10002-5
 435 MPa
@Temperature 500 °C
EN min.; EN 10002-5
 470 MPa
@Temperature 400 °C
EN min.; EN 10002-5
 475 MPa
@Temperature 300 °C
EN min.; EN 10002-5
 485 MPa
@Temperature 200 °C
EN min.; EN 10002-5
 525 MPa
@Temperature 100 °C
EN min.; EN 10002-5
 570 MPa
@Temperature 50.0 °C
EN min.; EN 10002-5
Tensile Strength, Yield 340 MPa
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 380 MPa
@Strain 1 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 110 MPa
@Strain 0.2 %,
Temperature 700 °C
EN min.
 120 MPa
@Strain 0.2 %,
Temperature 600 °C
EN min.; EN 10002-5
 130 MPa
@Strain 0.2 %,
Temperature 500 °C
EN min.; EN 10002-5
 135 MPa
@Strain 1 %,
Temperature 700 °C
EN min.
 140 MPa
@Strain 0.2 %,
Temperature 400 °C
EN min.; EN 10002-5
 150 MPa
@Strain 1 %,
Temperature 600 °C
EN min.; EN 10002-5
 150 MPa
@Strain 0.2 %,
Temperature 300 °C
EN min.; EN 10002-5
 160 MPa
@Strain 1 %,
Temperature 500 °C
EN min.; EN 10002-5
 165 MPa
@Strain 0.2 %,
Temperature 200 °C
EN min.; EN 10002-5
 170 MPa
@Strain 1 %,
Temperature 400 °C
EN min.; EN 10002-5
 180 MPa
@Strain 1 %,
Temperature 300 °C
EN min.; EN 10002-5
 195 MPa
@Strain 1 %,
Temperature 200 °C
EN min.; EN 10002-5
 200 MPa
@Strain 0.2 %,
Temperature 100 °C
EN min.; EN 10002-5
 235 MPa
@Strain 1 %,
Temperature 100 °C
EN min.; EN 10002-5
 245 MPa
@Strain 0.2 %,
Temperature 50.0 °C
EN min.; EN 10002-5
 280 MPa
@Strain 1 %,
Temperature 50.0 °C
EN min.; EN 10002-5
Elongation at Break 55 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Rupture Strength 4.00 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
 10.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
 16.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
 25.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
 41.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
 63.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 98.0 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
 157 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
 250 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
Modulus of Elasticity 200 GPaRT
 120 GPa
@Temperature 1000 °C
 163 GPa
@Temperature 500 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000840 ohm-cmRT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 18.2 µm/m-°C
@Temperature 500 °C
 19.5 µm/m-°C
@Temperature 1000 °C
Specific Heat Capacity 0.500 J/g-°CRT
 0.580 J/g-°C
@Temperature 500 °C
Thermal Conductivity 15.0 W/m-KRT
 21.2 W/m-K
@Temperature 500 °C
 29.0 W/m-K
@Temperature 1000 °C
Maximum Service Temperature, Air 1000 °CDry Air
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 900 °CStress Relief Annealing (min. 0.5 h)
 1020 - 1120 °CSolution Annealing
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.050 %
Cerium, Ce 1.3 %
Chromium, Cr 18.5 %
Iron, Fe 69.2 %
Nickel, Ni 9.5 %
Nitrogen, N 0.15 %
Silicon, Si 1.3 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Outokumpu 4318 Cr-Ni Austenitic Stainless Steel
Crucible Steel SUE52 Martensitic Steel
Outokumpu 4438 High Performance Austenitic Stainless Steel
Outokumpu 4541 Cr-Ni Austenitic Stainless Steel
Outokumpu 4571 Cr-Ni-Mo Austenitic Stainless Steel

NOUTOK42 / 18757

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.