MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Plenco 4349 Phenolic, Granular, Transfer Molded
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Novolac, Mineral Filled

Material Notes: PLENCO 04349 is a heat resistant, mineral filled phenolic molding compound offering optimized cure characteristics, and excellent heat resistant properties. PLENCO 04349 is also formulated to offer exceptional cosmetic characteristics in the molded product. UL recognized under component file E40654. 04349 is available in black.

Information supplied by Plenco.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.640 g/cc0.0231 lb/in³ASTM D1895
Density 1.56 g/cc0.0564 lb/in³ASTM D792
Water Absorption 0.118 %0.118 %ASTM D570
Linear Mold Shrinkage 0.0043 cm/cm0.0043 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 9191ASTM D785
Tensile Strength, Ultimate 51.0 MPa7400 psiASTM D638
Elongation at Break 0.71 %0.71 %ASTM D638
Tensile Modulus 9.40 GPa1360 ksiASTM D638
Flexural Strength 77.0 MPa11200 psiASTM D790
Flexural Modulus 9.10 GPa1320 ksiASTM D790
Compressive Strength 197 MPa28600 psiASTM D695
Izod Impact, Notched 0.155 J/cm0.290 ft-lb/inASTM D256
Charpy Impact, Notched 0.188 J/cm²0.895 ft-lb/in²ASTM D256
Impact 9797J/m Drop Ball Impact; PLENCO
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.90e+11 ohm-cm1.90e+11 ohm-cmASTM D247
Dielectric Constant 5.85.8ASTM D150
Dielectric Strength 11.1 kV/mm282 kV/inShort Time; ASTM D149
Dissipation Factor 0.0630.063ASTM D150
Arc Resistance 170 sec170 secASTM D495
Comparative Tracking Index 175 V175 VASTM D3638
 
Thermal PropertiesMetricEnglishComments
CTE, linear 38.0 µm/m-°C
@Temperature 40.0 - 130 °C
21.1 µin/in-°F
@Temperature 104 - 266 °F
TMA; ASTM E831
Maximum Service Temperature, Air 213 °C415 °FHeat Resistance; ASTM D570D
Deflection Temperature at 1.8 MPa (264 psi) 211 °C412 °FASTM D648
Flammability, UL94 V-1
@Thickness 1.50 mm
V-1
@Thickness 0.0591 in
Shrinkage 0.173 %0.173 %72 hr, 120ºC; ASTM D1299

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plenco 2000 Phenolic, Granular, Transfer Molded
Plenco 2000 Phenolic, Granular, Injection Molded
Plenco 2308 Phenolic, Granular, Transfer Molded
Plenco 2308 Phenolic, Granular, Injection Molded
Plenco 2311 Phenolic, Granular, Injection Molded

PLEL82 / 50654

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.