MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil Santoprene® 121-58W175 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A soft, black, UV resistant thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material combines good physical properties and chemical resistance, and is designed for thin wall or complex profile extrusion applications. This grade of Santoprene TPV is shear-dependent and can be processed on conventional thermoplastics equipment for extrusion. It is polyolefin based and completely recyclable.

Key Features:

  • Recommended for applications requiring excellent flex fatigue resistance.
  • Excellent ozone resistance.
  • Designed for improved UV resistance.
  • Designed for extruding thin sections with excellent definition (down to 0.33 mm [0.013"] radius). Long runs with minimal build-up of material on screen packs or narrow die sections.
  • EU and China RoHS compliant.
Applications:
  • Automotive- Weather Seals
Uses:
  • Automotive Applications
  • Automotive Interior Trim
Availability: Africa & Middle East, Europe, North America, Asia Pacific, Latin America and South America

Information provided by ExxonMobil Chemcial

Key Words: EU 2003/11/EC; RoHS Compliant
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 622 mm, 15 sec; ISO 868
 67Air at 302°F, 168 hr; ASTM D573
Tensile Strength at Break 653 psiAir at 302°F, 168 hr; ASTM D573
 725 psiAcross Flow; ASTM D412
Tensile Stress at Strain 305 psi
@Strain 100 %
Across Flow; ASTM D412
Elongation at Break 440 %Across Flow; ASTM D412
 475.2 %Air at 302°F, 168 hr; ASTM D573
Tear Strength 206 pli73°F, Die C; ASTM D624
Compression Set 18 %
@Temperature 22.8 °C,
Time 79200 sec
ASTM D395
 39 %
@Temperature 125 °C,
Time 252000 sec
ASTM D395
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 2.71.96 mm; ASTM D150
Dielectric Strength 650 V/mil2.03 mm; ASTM D149
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 275 °F
Brittleness Temperature -76.0 °FASTM D746
 
Processing PropertiesOriginal ValueComments
Processing Temperature 175 - 230 °C
Die Temperature 400 °FExtrusion
Melt Temperature 350 - 400 °FExtrusion
Drying Temperature 180 °F
Dry Time 3 hour
Back Pressure 725 - 2900 psiExtrusion
 
Descriptive Properties
ColorBlack
FormPellets

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ExxonMobil Santoprene® 121-67W175 Thermoplastic Elastomer
ExxonMobil Santoprene® 101-45W255 Thermoplastic Elastomer
ExxonMobil Santoprene® 121-50M100 Thermoplastic Elastomer
ExxonMobil Santoprene® 111-35 Thermoplastic Elastomer
ExxonMobil Santoprene® 101-64 Thermoplastic Elastomer

PADVA058 / 22748

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.