MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Röhm ACRYLITE PLUS® ZK-M Impact Acrylic Polymer  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, General Purpose, Molded; Acrylic, Heat Resistant, Molded; Acrylic, Impact Modified, Molded

Material Notes: ACRYLITE PLUS® ZK-M impact acrylic polymer is an amorphous, impact-modified thermoplastic molding and extrusion compound based on polymethyl methacrylate (PMMA).

Typical properties of ACRYLITE PLUS® impact acrylic polymers are high weather resistance, high light transmission, improved resistance to stress cracking, good melt flow rate, and easy to color.

The special properties of ACRYLITE PLUS ZK-M polymer are medium impact/break resistance and strength, low melt flow rate, high heat resistance, AMECA listed as ZKM (x), and FDA food contact use.

Application: Used for injection molded parts.

Information Provided by Evonik CYRO. The former Evonik Methacrylates business has been sold to Röhm (Roehm) GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Bulk Density 0.710 g/ccASTM D1895
Water Absorption at Saturation 0.30 %ASTM D570
Linear Mold Shrinkage 0.0030 - 0.0060 in/inASTM D955
Melt Flow 3.5 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 68ASTM D785
Tensile Strength at Break 8500 psiASTM D638
Elongation at Break 30 %ASTM D638
Elongation at Yield 5.0 %ASTM D638
Tensile Modulus 320000 psiASTM D638
Flexural Strength 13000 psiASTM D790
Flexural Modulus 320000 psiASTM D790
Izod Impact, Notched 0.500 ft-lb/in
@Temperature 0.000 °C
1/4" bar; ASTM D256
 0.850 ft-lb/in
@Temperature 23.0 °C
1/4" bar; ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 40.0 µin/in-°F
@Temperature 0.000 - 156 °C
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 196 °F
@Thickness 6.35 mm
Annealed; ASTM D648
Vicat Softening Point 210 °FASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze <= 1.0 %ASTM D1003
Yellow Index <= 0.30 %ASTM D1925
Transmission, Visible 91.5 %ASTM D1003
 
Processing PropertiesOriginal ValueComments
Middle Barrel Temperature 450 - 480 °F
Melt Temperature 450 - 480 °F
Mold Temperature 110 - 180 °F
Drying Temperature 180 °F
Dry Time 3 - 4 hour

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Röhm Acrylite® 8N Acrylic Polymer
Röhm Acrylite Plus® zdf Impact Acrylic Polymer
Röhm Acrylite Plus® zk3HR Impact Acrylic Polymer
Röhm Acrylite Plus® zk4BR Impact Acrylic Polymer
Röhm Acrylite Plus® zk4HR Impact Acrylic Polymer

PCYR00057 / 101046

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.