MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
A. Schulman Diamond Centrex® HGM Automotive Grade, Injection Molding Grade  (discontinued **)
Categories: Polymer; Thermoplastic; ASA Polymer

Material Notes: Centrex HGM resin is an exceptionally high-gloss grade of ASA (acrylonitrile-styrene-acrylate). This injection molding grade has excellent gloss retention, excellent resistance to chemicals and high heat, good resistance to weather aging, and a wide molding window.

Applications: Centrex HGM resin is used in the automotive market for exterior applications such as mirror housings, cowl grilles, license plate pockets, exterior trim and radiator grilles. As with any product, use of Centrex HGM resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

A. Schulman has acquired Network Polymers & Diamond Polymers.

Key Words: Weatherable Polymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.08 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0060 cm/cmASTM D955
Melt Flow 0.40 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 3.5 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 97ASTM D785
Tensile Strength, Yield 39.0 MPachs 0.2 in/min; ASTM D638
Tensile Modulus 2136 MPachs 0.2 in/min; ASTM D638
Flexural Strength 63.0 MPachs 0.05 in/min; ASTM D790
Flexural Modulus 2067 MPatangent; chs 0.05 in/min; ASTM D790
Izod Impact, Notched 21.0 J/m
@Thickness 3.17 mm,
Temperature -40.0 °C
ASTM D256
 208 J/m
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D256
Impact Test 1.10 J
@Temperature -40.0 °C
ASTM D3763
 30.0 J
@Temperature 23.0 °C
ASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear 121 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C0.125";; ASTM D648
 88.0 °C0.5";; ASTM D648
Vicat Softening Point 116 °C
@Load 1.00 kg
120°C/hr; ASTM D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
INEOS Styrolution Luran® S 778 UV Colored ASA
INEOS Styrolution Luran® S 777K ASA
INEOS Styrolution Luran® S 757G ASA
INEOS Styrolution Luran® S 778T ASA
INEOS Styrolution Luran® S 778 Q42 Colored ASA

PDIAM361 / 126452

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.