MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® 77G33L BK031 PA612-GF33
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612); Nylon 612, Glass Fiber Filler

Material Notes: 33% Glass Reinforced Polyamide 612

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.32 g/ccDAM; ISO 1183
Water Absorption 0.10 %
@Time 86400 sec
Immersion; DAM; Sim. to ISO 62
Moisture Absorption 0.700 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 100 cm³/gsulfuric acid 96%; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0030 cm/cmDAM; ISO 294-4, 2577
 0.0020 cm/cm
@Thickness 3.17 mm
Linear Mold Shrinkage, Transverse 0.0090 cm/cmDAM; ISO 294-4, 2577
 0.010 cm/cm
@Thickness 3.17 mm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 140 MPa50% RH; ISO 527-1/-2
 170 MPaDAM; ISO 527-1/-2
Elongation at Break 3.0 %DAM; ISO 527-1/-2
 3.2 %50% RH; ISO 527-1/-2
Tensile Modulus 7900 MPa50% RH; ISO 527-1/-2
 9500 MPaDAM; ISO 527-1/-2
Flexural Strength 250 MPaDAM; ISO 178
Flexural Modulus 8500 MPaDAM; ISO 178
Poissons Ratio 0.3450% RH
 0.34DAM
Izod Impact, Notched (ISO) 11.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 13.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Izod Impact, Unnotched (ISO) 60.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1U
Charpy Impact, Notched 12.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 13.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 VDAM; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 20.0 µm/m-°CDAM; ISO 11359-1/-2
 14.0 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
 26.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CDAM; ISO 11359-1/-2
 83.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 160 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
Melting Point 218 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 200 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 55.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 65.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 0.710 mm
DAM; IEC 60695-11-10
 HB
@Thickness 1.50 mm
DAM; IEC 60695-11-10
Flame Spread 23.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Glow Wire Ignition Temperature 700 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-13
 700 °C
@Thickness 1.50 mm
DAM; IEC 60695-2-13
 725 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-13
 
Processing PropertiesOriginal ValueComments
Melt Temperature 290 °COptimum, Injection
 280 - 300 °CRange, Injection
Mold Temperature 70.0 - 120 °CInjection
 100 °COptimum, Injection
Ejection Temperature 210 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging (mg)0.1G-value (condensate); ISO 6452; DAM
ISO designationISO 16396-PA612,GF33,M1CGR,S09-090
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>PA612-GF33<ISO 11469
PolymerPA612-GF33
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA612-GF33ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zytel® 151L NC010 PA612
Celanese Zytel® 153HSL NC010 PA612
Celanese Zytel® LC6200 BK385 PA612-HI
Celanese Zytel® 158 NC010 PA612
Celanese Zytel® 151 NC010 PA612

PDSX5367 / 198007

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.