MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 5140 Steel, annealed 830°C (1525°F)
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 5000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: The following are suggested consumables for arc welding processes: For 0.476 - 6.35 cm (3/16 - 2.5 in.) thicknesses - Manual Shielded Metal-Arc (AWS A5.5) Low Hydrogen Electrodes E11015, E11016, and E11018; Submerged Arc (AWS A5.23) F11x-Exxx; Gas Metal-Arc (AWS A5.28) ER110S; Flux Cored-Arc (AWS A5.29) E11xT. For 6.35 - 10.16 cm (2.5 - 4 in.) thicknesses - Manual Shielded Metal-Arc (AWS A5.5) Low Hydrogen Electrodes E11015, E11016, and E11018; Submerged Arc (AWS A5.23) F10x-Exxx; Gas Metal-Arc (AWS A5.28) ER100S; Flux Cored-Arc (AWS A5.29) E10xT.

Key Words: B.S. 530 A 40, B.S. 530 H 40, B.S. 530 M 40, B.S. 2 S 117, DIN 1.7035, AFNOR 42 C 4 (Fr), UNI 40 Cr 4 (Ital.), UNI 41 Cr 4 KB (Ital.), JIS SCr 4 H (Japan.), UNS G51400, ASTM A322, ASTM A331, ASTM A505, ASTM A519, SAE J404, SAE J412, SAE J770
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 167
Hardness, Knoop 188Converted from Brinell
Hardness, Rockwell B 85Converted from Brinell
Hardness, Vickers 175Converted from Brinell
Tensile Strength, Ultimate 570 MPa
Tensile Strength, Yield 295 MPa
Elongation at Break 28.6 %in 50mm.
Modulus of Elasticity 205 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel.
Poissons Ratio 0.29Calculated
Machinability 65 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPaTypical for steel
Izod Impact 41.0 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000228 ohm-cm
@Temperature 20.0 °C
 0.0000281 ohm-cm
@Temperature 100 °C
 0.0000352 ohm-cm
@Temperature 200 °C
 0.0000530 ohm-cm
@Temperature 400 °C
 0.0000785 ohm-cm
@Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.6 µm/m-°C
@Temperature 20.0 - 200 °C
 13.3 µm/m-°C
@Temperature 20.0 - 300 °C
 13.9 µm/m-°C
@Temperature 20.0 - 400 °C
 14.0 µm/m-°C
@Temperature 20.0 - 500 °C
 14.6 µm/m-°C
@Temperature 20.0 - 600 °C
 14.9 µm/m-°C
@Temperature 20.0 - 700 °C
Specific Heat Capacity 0.452 J/g-°C
@Temperature >=100 °C
 0.473 J/g-°C
@Temperature 20.0 - 200 °C
 0.519 J/g-°C
@Temperature 20.0 - 400 °C
Thermal Conductivity 31.3 W/m-K
@Temperature 600 °C
 37.7 W/m-K
@Temperature 400 °C
 43.4 W/m-K
@Temperature 200 °C
 44.6 W/m-K
@Temperature 100 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.38 - 0.43 %
Chromium, Cr 0.70 - 0.90 %
Iron, Fe 97.395 - 98.07 %As remainder
Manganese, Mn 0.70 - 0.90 %
Phosphorus, P <= 0.035 %
Silicon, Si 0.15 - 0.30 %
Sulfur, S <= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 5140 Steel, oil quenched 845°C (1550°F), 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 5140 Steel, normalized 870°C (1600°F)
AISI 5140 Steel, annealed 830°C (1525°F), 25 mm (1 in.) round
AISI 4340 Steel, annealed, 25 mm round
AISI 5140 Steel, normalized, 13 mm (0.5 in.) round

M514AG / 8071

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.