MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Ultramid® FRee A3U40G5 25% Glass Filled PA66 FR (Conditioned)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: Flame retardant without halogens and red phosphorus, 25% glass fiber reinforced injection-molding grade; light colorable; outstanding mechanical and electrical properties.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.42 g/cc0.0513 lb/in³ISO 1183
Moisture Absorption at Equilibrium 1.1 - 1.5 %1.1 - 1.5 %23°C; 50% RH; ISO 62
Water Absorption at Saturation 4.0 - 4.6 %4.0 - 4.6 %ISO 62
Linear Mold Shrinkage 0.0040 cm/cm0.0040 in/inrestricted
Melt Flow 42.6 g/10 min
@Load 5.00 kg,
Temperature 275 °C
42.6 g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 140 MPa20300 psi50 mm/min; ISO 527-1/-2
Elongation at Yield 3.8 %3.8 %50 mm/min; ISO 527-1/-2
Modulus of Elasticity 7.40 GPa1070 ksiISO 527-1/-2
Flexural Strength 160 MPa23200 psiat max force; ISO 178
Flexural Modulus 7.40 GPa1070 ksiISO 178
Izod Impact, Notched (ISO) 9.00 kJ/m²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 180/A
Charpy Impact Unnotched 6.00 J/cm²
@Temperature 23.0 °C
28.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant 4.6
@Frequency 1e+6 Hz
4.6
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.10
@Frequency 1e+6 Hz
0.10
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VTest solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 260 °C500 °FDIN 53765
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 - 300 °C536 - 572 °FInjection-molding/Extrusion
Mold Temperature 80.0 - 90.0 °C176 - 194 °FInjection-molding
 
Descriptive Properties
Commercial StatusEurope

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® FRee A3U40G5 25% Glass Filled PA66 FR (Dry)
BASF Ultramid® A3UG5 BK 23260 25% Glass Filled PA66 (Dry)

PBASG0306 / 131939

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.