MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Meldin Supplier

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Vespel® CR-6110 Carbon-Reinforced Fluoropolymer
Categories: Polymer; Thermoplastic; Fluoropolymer

Material Notes: DuPont™ Vespel® CR-6110 shapes are carbon-fiber filled thermoplastic fluoropolymers that have demonstrated outstanding performance in aggressive wet chemical / plasma conditions and elevated temperatures. Customers report improved preventative maintenance cycles by switching to Vespel® CR-6110 in wafer cleaning and resist stripping operations. It has also demonstrated good ultraviolet (UV) resistance in Flat Panel Display applications. In dry plasma applications, Vespel® CR-6110 has been used as a thermal insulator and bearing. Vespel® CR-6110 is available upon request in wide variety of shapes (plaque, sheet, rod, ring, tube) and can also be machined for custom parts in various applications.

Information provided by DuPont. This product line has remained with DuPont after the DuPont-Dow merger.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.06 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 111 kgf, x-y; ASTM E384
 141 kgf, z; ASTM E384
Tensile Strength 15.0 MPaz; ASTM D3039
 126 MPax-y; ASTM D3039
Elongation at Break 0.70 %z; ASTM D3039
 1.4 %x-y; ASTM D3039
Tensile Modulus 2287 MPaz; ASTM D3039
 7180 MPax-y; ASTM D3039
Flexural Strength 180 MPax-y; ASTM D790
Flexural Modulus 12100 MPax-y; ASTM D790
Compressive Strength 25.0 MPa
@Temperature 260 °C
x-y; ASTM D695
 103 MPa
@Temperature 22.8 °C
x-y; ASTM D695
 131 MPa
@Temperature 260 °C
z; ASTM D695
 189 MPa
@Temperature 22.8 °C
z; ASTM D695
Compressive Modulus 1137 MPa
@Temperature 260 °C
z; ASTM D695
 1785 MPa
@Temperature 260 °C
x-y; ASTM D695
 2810 MPa
@Temperature 22.8 °C
z; ASTM D695
 10045 MPa
@Temperature 22.8 °C
x-y; ASTM D695
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 0.010 ohm-cmx-y; JIS K7194
 0.10 ohm-cmx-y; JIS K7194
Surface Resistivity per Square 0.10 ohmx-y; JIS K7194
 0.10 ohmx-y; JIS K7194
 
Thermal PropertiesOriginal ValueComments
CTE, linear 5.60 µm/m-°C
@Temperature 23.0 - 260 °C
x-y; ASTM E831
 290 µm/m-°C
@Temperature 35.0 - 149 °C
z; ASTM E831
 450 µm/m-°C
@Temperature 149 - 204 °C
z; ASTM E831
 720 µm/m-°C
@Temperature 204 - 260 °C
z; ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 319 °Cx-y; ASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® CR-6100 Carbon-Reinforced Fluoropolymer
DuPont Mobility and Materials Vespel® CP-0644 Polyimide
DuPont Mobility and Materials Vespel® CP-8000 Polyimide
Hexcel® Fibrelam® 2000 Grade 5 Panels for Aircraft Flooring
BASF Ultraform® N2320 U035 POM

PDTA7747e / 183709

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.